MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

EMS-Grivory Grilamid® 2S 25 W 20 HL X black 9992 PA610
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 610 (PA610)

Material Notes: Product Description: Grilamid 2S 25 W 20 HL X black 9992 is a semi-flexible high viscosity heat stabilized, impact modified and plasticized Polyamide 610, especially suitable for extrusion applications. This PA610 product is to a large extent based on renewable raw materials and its eco-profile is very favorable when compared to similar products based on crude oil. The main features of Grilamid 2S 25 W 20 HL X black 9992 are:
  • High impact strength, even at low temperatures
  • High heat resistance
  • Good chemical resistance
  • Easy processing
Application examples: Preferred applications are tubes in the fields of Automotive and Industry components, whereas the product is not recommended for direct permanent contact with gasoline.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.03 g/cc0.0372 lb/in³Dry; ISO 1183
Water Absorption 3.0 %3.0 %Sim. to ISO 62
Moisture Absorption 0.500 %0.500 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.018 cm/cm0.018 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.013 cm/cm0.013 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 35.0 MPa5080 psiConditioned; ISO 2039-1
 50.0 MPa7250 psiDry; ISO 2039-1
Tensile Strength at Break 50.0 MPa7250 psiDry; ISO 527-1/-2
 50.0 MPa7250 psiConditioned; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Dry; ISO 527-1/-2
 >= 50 %>= 50 %Conditioned; ISO 527-1/-2
Tensile Modulus 0.450 GPa65.3 ksiConditioned; ISO 527-1/-2
 0.750 GPa109 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  1.50 J/cm²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 1.50 J/cm²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+9 ohm-cm1.00e+9 ohm-cmDry; IEC 60093
 1.00e+10 ohm-cm1.00e+10 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 36.0 kV/mm914 kV/inDry; IEC 60243-1
 36.0 kV/mm914 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 200 µm/m-°C111 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 150 µm/m-°C83.3 µin/in-°FISO 11359-1/-2
Melting Point 215 °C419 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 130 °C266 °FLong Term; ISO 2578
 170 °C338 °FShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 100 °C212 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °C122 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AdditivesPlasticizer
AutomotiveAir intake systems
 Compressed air systems
 Hydraulic systems
Electricals & ElectronicsCables & Tubes
FormGranules
Industry & Consumer goodsHydraulics & Pneumatics
ProcessingOther Extrusion
 Profile Extrusion
Product AttributesBio based Polyamide
 Flexible
 High viscosity
Special CharacteristicsHigh impact or impact modified
 Improved heat resistance
 Light stabilized or stable to light

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
303 Stainless Steel, annealed bar
EMS-Grivory Grilamid® 1SVX-50H black 9288 PA1010-GF50
EMS-Grivory Grilamid® 1S XE 4224 nat PA1010
Aluminum 6061-T6; 6061-T651

PGRH013 / 156722

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.