MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 282® Nickel Alloy Sheet, Gamma-Prime Strengthened
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Excellent High Temperature Strength

HAYNES® 282® alloy is a wrought, gamma-prime strengthened superalloy developed for high temperature structural applications, especially those in aero and land-based gas turbine engines. It possesses a unique combination of creep strength, thermal stability, weldability, and fabricability. The alloy has excellent creep strength in the temperature range of 1200 to 1700°F (649 to 927°C), surpassing that of Waspaloy alloy, and approaching that of R-41 alloy.

Easily Fabricated: This high level of creep strength in HAYNES 282 alloy has been attained at a relatively low volume fraction of the strengthening gamma-prime phase, resulting in outstanding resistance to strain-age cracking (normally a problem with superalloys in this creep strength range). Additionally, slow gamma-prime precipitation kinetics allow for the alloy to have excellent ductility in the as-annealed condition. Consequently, HAYNES 282 alloy exhibits superior weldability and fabricability.

Product Forms: HAYNES 282 alloy is designed for use in the form of plate, sheet, strip, foil, billet, bar, wire welding products, pipe, and tubing.

Heat Treatment: HAYNES 282 alloy is provided in the solution-annealed condition, in which it is readily formable. The typical solution annealing temperature is in the range of 2050 to 2100°F (1121 to 1149°C). After component fabrication, a two-step age hardening treatment is required to put the alloy into the high-strength condition. The treatment includes 1850°F (1010°C) / 2 hours / AC (air cool) + 1450°F (788°C) / 8 hours / AC.

Applications: Suitable for critical gas turbine applications, such as sheet fabrications, seamless and flash butt-welded rings, and cases found in compressor, combustor, and turbine sections. In augmented aircraft gas turbines, it is useful for exhaust and nozzle components. In land-based gas turbines, HAYNES 282 alloy is a good candidate for transition sections and other hot-gas-path components.

Machining: HAYNES 282 alloy has similar machining characteristics to other nickel alloys used at high temperatures. Rough machining should be carried out prior to age-hardening, using the following guidelines. Final machining or finish grinding may be done after age-hardening.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.27 g/cc0.299 lb/in³Solution Annealed
 8.29 g/cc0.299 lb/in³Age-hardened
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  975 MPa
@Treatment Temp. 871 °C,
Time 3.60e+6 sec
141000 psi
@Treatment Temp. 1600 °F,
Time 1000 hour
Room temp test after thermal exposure
 1102 MPa
@Treatment Temp. 816 °C,
Time 3.60e+6 sec
159800 psi
@Treatment Temp. 1500 °F,
Time 1000 hour
Room temp test after thermal exposure
 1176 MPa
@Treatment Temp. 760 °C,
Time 3.60e+6 sec
170600 psi
@Treatment Temp. 1400 °F,
Time 1000 hour
Room temp test after thermal exposure
 1191 MPa
@Treatment Temp. 649 °C,
Time 3.60e+6 sec
172700 psi
@Treatment Temp. 1200 °F,
Time 1000 hour
Room temp test after thermal exposure
Tensile Strength, Yield  502 MPa
@Treatment Temp. 502 °C,
Time 3.60e+6 sec
72800 psi
@Treatment Temp. 936 °F,
Time 1000 hour
0.2%. Room temp test after thermal exposure
 634 MPa
@Treatment Temp. 634 °C,
Time 3.60e+6 sec
92000 psi
@Treatment Temp. 1170 °F,
Time 1000 hour
0.2%. Room temp test after thermal exposure
 718 MPa
@Treatment Temp. 718 °C,
Time 3.60e+6 sec
104000 psi
@Treatment Temp. 1320 °F,
Time 1000 hour
0.2%. Room temp test after thermal exposure
 778 MPa
@Treatment Temp. 778 °C,
Time 3.60e+6 sec
113000 psi
@Treatment Temp. 1430 °F,
Time 1000 hour
0.2%. Room temp test after thermal exposure
Elongation at Break  22.3 %
@Treatment Temp. 634 °C,
Time 3.60e+6 sec
22.3 %
@Treatment Temp. 1170 °F,
Time 1000 hour
Room temp test after thermal exposure
 22.8 %
@Treatment Temp. 718 °C,
Time 3.60e+6 sec
22.8 %
@Treatment Temp. 1320 °F,
Time 1000 hour
Room temp test after thermal exposure
 24.2 %
@Treatment Temp. 502 °C,
Time 3.60e+6 sec
24.2 %
@Treatment Temp. 936 °F,
Time 1000 hour
Room temp test after thermal exposure
 25.8 %
@Treatment Temp. 778 °C,
Time 3.60e+6 sec
25.8 %
@Treatment Temp. 1430 °F,
Time 1000 hour
Room temp test after thermal exposure
Creep Strength  34.0 MPa
@Temperature 927 °C,
Time 3.60e+6 sec
4930 psi
@Temperature 1700 °F,
Time 1000 hour
1% Creep
 62.0 MPa
@Temperature 927 °C,
Time 360000 sec
8990 psi
@Temperature 1700 °F,
Time 100 hour
1% Creep
 69.0 MPa
@Temperature 871 °C,
Time 3.60e+6 sec
10000 psi
@Temperature 1600 °F,
Time 1000 hour
1% Creep
 124 MPa
@Temperature 871 °C,
Time 360000 sec
18000 psi
@Temperature 1600 °F,
Time 100 hour
1% Creep
 145 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
21000 psi
@Temperature 1500 °F,
Time 1000 hour
1% Creep
 221 MPa
@Temperature 816 °C,
Time 360000 sec
32100 psi
@Temperature 1500 °F,
Time 100 hour
1% Creep
 241 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
35000 psi
@Temperature 1400 °F,
Time 1000 hour
1% Creep
 331 MPa
@Temperature 760 °C,
Time 360000 sec
48000 psi
@Temperature 1400 °F,
Time 100 hour
1% Creep
 365 MPa
@Temperature 704 °C,
Time 3.60e+6 sec
52900 psi
@Temperature 1300 °F,
Time 1000 hour
1% Creep
 496 MPa
@Temperature 704 °C,
Time 360000 sec
71900 psi
@Temperature 1300 °F,
Time 100 hour
1% Creep
 545 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
79000 psi
@Temperature 1200 °F,
Time 1000 hour
1% Creep
Rupture Strength  41.0 MPa
@Temperature 927 °C,
Time 3.60e+6 sec
5950 psi
@Temperature 1700 °F,
Time 1000 hour
 83.0 MPa
@Temperature 927 °C,
Time 360000 sec
12000 psi
@Temperature 1700 °F,
Time 100 hour
 83.0 MPa
@Temperature 871 °C,
Time 3.60e+6 sec
12000 psi
@Temperature 1600 °F,
Time 1000 hour
 152 MPa
@Temperature 871 °C,
Time 360000 sec
22000 psi
@Temperature 1600 °F,
Time 100 hour
 159 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
23100 psi
@Temperature 1500 °F,
Time 1000 hour
 255 MPa
@Temperature 816 °C,
Time 360000 sec
37000 psi
@Temperature 1500 °F,
Time 100 hour
 262 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
38000 psi
@Temperature 1400 °F,
Time 1000 hour
 386 MPa
@Temperature 760 °C,
Time 360000 sec
56000 psi
@Temperature 1400 °F,
Time 100 hour
 386 MPa
@Temperature 704 °C,
Time 3.60e+6 sec
56000 psi
@Temperature 1300 °F,
Time 1000 hour
 517 MPa
@Temperature 704 °C,
Time 360000 sec
75000 psi
@Temperature 1300 °F,
Time 100 hour
 552 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
80100 psi
@Temperature 1200 °F,
Time 1000 hour
Modulus of Elasticity  140 GPa
@Temperature 1000 °C
20300 ksi
@Temperature 1830 °F
Dynamic
 154 GPa
@Temperature 900 °C
22300 ksi
@Temperature 1650 °F
Dynamic
 166 GPa
@Temperature 800 °C
24100 ksi
@Temperature 1470 °F
Dynamic
 175 GPa
@Temperature 700 °C
25400 ksi
@Temperature 1290 °F
Dynamic
 183 GPa
@Temperature 600 °C
26500 ksi
@Temperature 1110 °F
Dynamic
 190 GPa
@Temperature 500 °C
27600 ksi
@Temperature 932 °F
Dynamic
 196 GPa
@Temperature 400 °C
28400 ksi
@Temperature 752 °F
Dynamic
 202 GPa
@Temperature 300 °C
29300 ksi
@Temperature 572 °F
Dynamic
 209 GPa
@Temperature 200 °C
30300 ksi
@Temperature 392 °F
Dynamic
 213 GPa
@Temperature 100 °C
30900 ksi
@Temperature 212 °F
Dynamic
 217 GPa
@Temperature 25.0 °C
31500 ksi
@Temperature 77.0 °F
Dynamic
Poissons Ratio  0.319
@Temperature 25.0 °C
0.319
@Temperature 77.0 °F
 0.326
@Temperature 100 °C
0.326
@Temperature 212 °F
 0.335
@Temperature 200 °C
0.335
@Temperature 392 °F
 0.335
@Temperature 300 °C
0.335
@Temperature 572 °F
 0.337
@Temperature 400 °C
0.337
@Temperature 752 °F
 0.341
@Temperature 500 °C
0.341
@Temperature 932 °F
 0.346
@Temperature 600 °C
0.346
@Temperature 1110 °F
 0.352
@Temperature 700 °C
0.352
@Temperature 1290 °F
 0.355
@Temperature 800 °C
0.355
@Temperature 1470 °F
 0.357
@Temperature 900 °C
0.357
@Temperature 1650 °F
 0.363
@Temperature 1000 °C
0.363
@Temperature 1830 °F
Shear Modulus  51.0 GPa
@Temperature 1000 °C
7400 ksi
@Temperature 1830 °F
Dynamic
 57.0 GPa
@Temperature 900 °C
8270 ksi
@Temperature 1650 °F
Dynamic
 61.0 GPa
@Temperature 800 °C
8850 ksi
@Temperature 1470 °F
Dynamic
 65.0 GPa
@Temperature 700 °C
9430 ksi
@Temperature 1290 °F
Dynamic
 68.0 GPa
@Temperature 600 °C
9860 ksi
@Temperature 1110 °F
Dynamic
 71.0 GPa
@Temperature 500 °C
10300 ksi
@Temperature 932 °F
Dynamic
 73.0 GPa
@Temperature 400 °C
10600 ksi
@Temperature 752 °F
Dynamic
 76.0 GPa
@Temperature 300 °C
11000 ksi
@Temperature 572 °F
Dynamic
 78.0 GPa
@Temperature 200 °C
11300 ksi
@Temperature 392 °F
Dynamic
 80.0 GPa
@Temperature 100 °C
11600 ksi
@Temperature 212 °F
Dynamic
 82.0 GPa
@Temperature 25.0 °C
11900 ksi
@Temperature 77.0 °F
Dynamic
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0001261 ohm-cm
@Temperature 25.0 °C
0.0001261 ohm-cm
@Temperature 77.0 °F
 0.0001278 ohm-cm
@Temperature 100 °C
0.0001278 ohm-cm
@Temperature 212 °F
 0.0001299 ohm-cm
@Temperature 200 °C
0.0001299 ohm-cm
@Temperature 392 °F
 0.0001299 ohm-cm
@Temperature 1000 °C
0.0001299 ohm-cm
@Temperature 1830 °F
 0.0001318 ohm-cm
@Temperature 300 °C
0.0001318 ohm-cm
@Temperature 572 °F
 0.0001326 ohm-cm
@Temperature 900 °C
0.0001326 ohm-cm
@Temperature 1650 °F
 0.0001334 ohm-cm
@Temperature 400 °C
0.0001334 ohm-cm
@Temperature 752 °F
 0.0001345 ohm-cm
@Temperature 800 °C
0.0001345 ohm-cm
@Temperature 1470 °F
 0.000135 ohm-cm
@Temperature 500 °C
0.000135 ohm-cm
@Temperature 932 °F
 0.0001355 ohm-cm
@Temperature 700 °C
0.0001355 ohm-cm
@Temperature 1290 °F
 0.0001362 ohm-cm
@Temperature 600 °C
0.0001362 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.1 µm/m-°C
@Temperature 25.0 - 100 °C
6.72 µin/in-°F
@Temperature 77.0 - 212 °F
 12.4 µm/m-°C
@Temperature 25.0 - 200 °C
6.89 µin/in-°F
@Temperature 77.0 - 392 °F
 12.8 µm/m-°C
@Temperature 25.0 - 300 °C
7.11 µin/in-°F
@Temperature 77.0 - 572 °F
 13.1 µm/m-°C
@Temperature 25.0 - 400 °C
7.28 µin/in-°F
@Temperature 77.0 - 752 °F
 13.5 µm/m-°C
@Temperature 25.0 - 500 °C
7.50 µin/in-°F
@Temperature 77.0 - 932 °F
 13.7 µm/m-°C
@Temperature 25.0 - 600 °C
7.61 µin/in-°F
@Temperature 77.0 - 1110 °F
 14.2 µm/m-°C
@Temperature 25.0 - 700 °C
7.89 µin/in-°F
@Temperature 77.0 - 1290 °F
 14.9 µm/m-°C
@Temperature 25.0 - 800 °C
8.28 µin/in-°F
@Temperature 77.0 - 1470 °F
 15.9 µm/m-°C
@Temperature 25.0 - 900 °C
8.83 µin/in-°F
@Temperature 77.0 - 1650 °F
 16.9 µm/m-°C
@Temperature 25.0 - 1000 °C
9.39 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity  0.436 J/g-°C
@Temperature 25.0 °C
0.104 BTU/lb-°F
@Temperature 77.0 °F
 0.463 J/g-°C
@Temperature 100 °C
0.111 BTU/lb-°F
@Temperature 212 °F
 0.494 J/g-°C
@Temperature 200 °C
0.118 BTU/lb-°F
@Temperature 392 °F
 0.522 J/g-°C
@Temperature 300 °C
0.125 BTU/lb-°F
@Temperature 572 °F
 0.544 J/g-°C
@Temperature 400 °C
0.130 BTU/lb-°F
@Temperature 752 °F
 0.563 J/g-°C
@Temperature 500 °C
0.135 BTU/lb-°F
@Temperature 932 °F
 0.581 J/g-°C
@Temperature 600 °C
0.139 BTU/lb-°F
@Temperature 1110 °F
 0.594 J/g-°C
@Temperature 700 °C
0.142 BTU/lb-°F
@Temperature 1290 °F
 0.650 J/g-°C
@Temperature 800 °C
0.155 BTU/lb-°F
@Temperature 1470 °F
 0.668 J/g-°C
@Temperature 900 °C
0.160 BTU/lb-°F
@Temperature 1650 °F
 0.676 J/g-°C
@Temperature 1000 °C
0.162 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity  10.3 W/m-K
@Temperature 25.0 °C
71.5 BTU-in/hr-ft²-°F
@Temperature 77.0 °F
 12.0 W/m-K
@Temperature 100 °C
83.3 BTU-in/hr-ft²-°F
@Temperature 212 °F
 14.1 W/m-K
@Temperature 200 °C
97.9 BTU-in/hr-ft²-°F
@Temperature 392 °F
 16.3 W/m-K
@Temperature 300 °C
113 BTU-in/hr-ft²-°F
@Temperature 572 °F
 18.5 W/m-K
@Temperature 400 °C
128 BTU-in/hr-ft²-°F
@Temperature 752 °F
 20.5 W/m-K
@Temperature 500 °C
142 BTU-in/hr-ft²-°F
@Temperature 932 °F
 22.6 W/m-K
@Temperature 600 °C
157 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 24.8 W/m-K
@Temperature 700 °C
172 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 26.1 W/m-K
@Temperature 800 °C
181 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 27.3 W/m-K
@Temperature 900 °C
189 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 28.9 W/m-K
@Temperature 1000 °C
201 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1300 - 1375 °C2370 - 2507 °F
Solidus 1300 °C2370 °F
Liquidus 1375 °C2507 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 1120 - 1150 °C2050 - 2100 °FTypical for solution annealing
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 1.5 %1.5 %
Boron, B 0.0050 %0.0050 %
Carbon, C 0.060 %0.060 %
Chromium, Cr 20 %20 %
Cobalt, Co 10 %10 %
Iron, Fe <= 1.5 %<= 1.5 %
Manganese, Mn <= 0.30 %<= 0.30 %
Molybdenum, Mo 8.5 %8.5 %
Nickel, Ni 57 %57 %as balance
Silicon, Si <= 0.15 %<= 0.15 %
Titanium, Ti 2.1 %2.1 %
 
Descriptive Properties
Thermal Diffusivity0.0288 cm2/s25°C
 0.0315 cm2/s100°C
 0.0348 cm2/s200°C
 0.0381 cm2/s300°C
 0.0413 cm2/s400°C
 0.0444 cm2/s500°C
 0.0473 cm2/s600°C
 0.0488 cm2/s800°C
 0.0498 cm2/s900°C
 0.0509 cm2/s700°C
 0.0521 cm2/s1000°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes 282® Nickel Alloy Sheet, Solution Annealed and Age-hardened
Haynes 282® Nickel Alloy Sheet, Plate and Bar, Solution Annealed
Haynes 242® alloy, cold rolled sheet, annealed and aged
446 Stainless Steel, Annealed Strip
Special Metals INCONEL® Alloy 625

NHAY989 / 162653

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.