MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ascend Performance Materials Vydyne® R533 NAT Nylon 66, 33% Glass Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Vydyne R533 NAT is a general purpose, 33% glass-filled, high viscosity PA66 based resin designed for injection molding applications. R533 NAT offers standard flow with a natural surface finish and maintains the excellent resistance typical of PA66 in chemicals, machine and motor oils, solvents, and gasoline.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc0.0506 lb/in³DAM; ISO 1183
Water Absorption 0.80 %
@Time 86400 sec
0.80 %
@Time 24.0 hour
DAM; ISO 62
Moisture Absorption at Equilibrium 1.7 %1.7 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cm
@Thickness 2.00 mm
0.0040 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm
@Thickness 2.00 mm
0.0090 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 145 MPa21000 psi50% RH; ISO 527-2
 205 MPa29700 psiDAM; ISO 527-2
Elongation at Break 3.0 %3.0 %DAM; ISO 527-2
 5.0 %5.0 %50% RH; ISO 527-2
Tensile Modulus 7.90 GPa1150 ksi50% RH; ISO 527-2
 10.6 GPa1540 ksiDAM; ISO 527-2
Flexural Strength 200 MPa29000 psi50% RH; ISO 178
 290 MPa42100 psiDAM; ISO 178
Flexural Modulus 6.50 GPa943 ksi50% RH; ISO 178
 10.2 GPa1480 ksiDAM; ISO 178
Poissons Ratio 0.400.40ISO 527-2
Izod Impact, Notched (ISO)  10.0 kJ/m²
@Temperature -40.0 °C
4.76 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 11.0 kJ/m²
@Temperature -40.0 °C
5.23 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 180/1A
 12.0 kJ/m²
@Temperature -30.0 °C
5.71 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 12.0 kJ/m²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 16.0 kJ/m²
@Temperature 23.0 °C
7.61 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Charpy Impact Unnotched  6.90 J/cm²
@Temperature -40.0 °C
32.8 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eU
 7.10 J/cm²
@Temperature -30.0 °C
33.8 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
 7.50 J/cm²
@Temperature -40.0 °C
35.7 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eU
 7.70 J/cm²
@Temperature -30.0 °C
36.6 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
 8.60 J/cm²
@Temperature 23.0 °C
40.9 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eU
Charpy Impact, Notched  1.10 J/cm²
@Temperature -40.0 °C
5.23 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eA
 1.10 J/cm²
@Temperature -40.0 °C
5.23 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 1.30 J/cm²
@Temperature 23.0 °C
6.19 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 1.70 J/cm²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm
@Thickness 1.00 mm
1.00e+14 ohm-cm
@Thickness 0.0394 in
DAM; IEC 60093
Dielectric Strength 20.0 kV/mm
@Thickness 1.00 mm
508 kV/in
@Thickness 0.0394 in
DAM; IEC 60243
Arc Resistance 120 - 180 sec
@Thickness 3.00 mm
120 - 180 sec
@Thickness 0.118 in
PLC 5; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
600 V
@Thickness 0.118 in
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 7.0 - 15 sec7.0 - 15 secPLC 4; UL 746
 15 - 30 sec15 - 30 secPLC 3; UL 746
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
 >= 120 arcs>= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/min0.394 - 1.00 in/minPLC 1; UL 746
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 21.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
11.7 µin/in-°F
@Thickness 0.0787 in,
Temperature 95.0 - 131 °F
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 106 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
58.9 µin/in-°F
@Thickness 0.0787 in,
Temperature 73.4 - 131 °F
DAM; ISO 11359-2
Melting Point 260 °C500 °FDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 260 °C500 °FUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 250 °C482 °FUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical  120 °C
@Thickness 0.750 mm
248 °F
@Thickness 0.0295 in
UL 746
 120 °C
@Thickness 1.50 mm
248 °F
@Thickness 0.0591 in
UL 746
 120 °C
@Thickness 3.00 mm
248 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical with Impact  100 °C
@Thickness 0.750 mm
212 °F
@Thickness 0.0295 in
UL 746
 100 °C
@Thickness 1.50 mm
212 °F
@Thickness 0.0591 in
UL 746
 105 °C
@Thickness 3.00 mm
221 °F
@Thickness 0.118 in
UL 746
UL RTI, Mechanical without Impact  125 °C
@Thickness 0.750 mm
257 °F
@Thickness 0.0295 in
UL 746
 125 °C
@Thickness 1.50 mm
257 °F
@Thickness 0.0591 in
UL 746
 125 °C
@Thickness 3.00 mm
257 °F
@Thickness 0.118 in
UL 746
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Glow Wire Ignition Temperature  725 °C
@Thickness 1.50 mm
1340 °F
@Thickness 0.0591 in
IEC 60695-2-13
 750 °C
@Thickness 3.00 mm
1380 °F
@Thickness 0.118 in
IEC 60695-2-13
 775 °C
@Thickness 0.750 mm
1430 °F
@Thickness 0.0295 in
IEC 60695-2-13
Glow Wire Flammability Index  725 °C
@Thickness 1.50 mm
1340 °F
@Thickness 0.0591 in
IEC 60695-2-12
 750 °C
@Thickness 0.750 mm
1380 °F
@Thickness 0.0295 in
IEC 60695-2-12
 800 °C
@Thickness 3.00 mm
1470 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Middle Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Front Barrel Temperature 280 - 310 °C536 - 590 °FInjection
Nozzle Temperature 280 - 310 °C536 - 590 °FInjection
Melt Temperature 285 - 305 °C545 - 581 °FInjection
Mold Temperature 65.0 - 95.0 °C149 - 203 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 4.00 hour4.00 hourInjection
 
Descriptive Properties
AdditiveLubricant
Agency RatingsASTM, D4066 PA011G35
 ASTM, D6779 PA011G35
 EC, 1935/2004
 EU, 10/2011
 EU, 2023/2006
 FDA, 21 CFR 177.1500
 NSF, STD-51
AppearanceNatural Color
Automotive Material SpecificationChrysler MS-DB-41_CPN 1853
FeaturesChemical Resistant
 Corrosion Resistant
 Good Dimensional Stability
 Good Electrical Properties
 Good Flow
 Good Mold Release
 High Rigidity
 High Strength
 Lubricated
 Non-Corrosive
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman SCHULAMID® 6 GF33 33% Glass Fiber Reinforced Nylon 6
PTS Trimid® N66-G33 33% Glass Fiber Reinforced Nylon 6/6
Chase Plastics CP Pryme® NN133L (Dry) Nylon 66, 33% Glass Fiber Reinforced, Lubricated
Niche Polymer PA66GF33N Nylon 66, 33% Glass Fiber Filled
Polymer Resources NY66-G33 Nylon 66, 33% Glass Reinforced

PASCE9812 / 220913

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.