MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Stellarchem MP-950NC TPE Compound
Categories: Polymer; Thermoplastic; Elastomer, TPE; Olefinic TPE

Material Notes: This grade of Stellarchem TPE is shear dependent and can be processed on conventional thermoplastics equipment for injection molding or extrusion. It's a soft, elastomeric polyolefin based, completely recyclable, colorable & non-hygroscopic thermoplastics elastomer material.

Information provided by Stellarchem Polymer & Industrial

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³
Particle Mesh Size 80 - 150 Mesh80 - 150 Mesh
Melt Flow 47.94 g/10 min47.94 g/10 minJIS K7210
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 5353JIS K6301
Tensile Strength, Ultimate 5.88 MPa853 psiJIS K6301
Elongation at Break 678 %678 %JIS K6301
100% Modulus 4.90 MPa
@Strain 100 %
711 psi
@Strain 100 %
JIS K6301
300% Modulus 0.392 MPa
@Strain 300 %
56.9 psi
@Strain 300 %
JIS K6301
Tear Strength 37.7 kN/m215 pliJIS K6301-B
 
Processing PropertiesMetricEnglishComments
Processing Temperature 200 - 220 °C392 - 428 °FMetering Temperature, Extrusion
Rear Barrel Temperature 160 - 180 °C320 - 356 °FExtrusion
 160 - 180 °C320 - 356 °FInjection Molding
Middle Barrel Temperature 180 - 200 °C356 - 392 °FTransition, Extrusion
 180 - 200 °C356 - 392 °FInjection Molding
Front Barrel Temperature 200 - 220 °C392 - 428 °FInjection Molding
 220 - 230 °C428 - 446 °FExtrusion
Nozzle Temperature 220 - 230 °C428 - 446 °FInjection Molding
Die Temperature 195 - 210 °C383 - 410 °FExtrusion
Melt Temperature 150 - 230 °C302 - 446 °FExtrusion
 150 - 230 °C302 - 446 °FInjection Molding
Mold Temperature 25.0 - 40.0 °C77.0 - 104 °FInjection Molding
Injection Pressure 5.00 - 40.0 MPa725 - 5800 psiInjection Molding
Back Pressure 0.500 - 1.00 MPa72.5 - 145 psiInjection Molding
Screw Speed 60 - 100 rpm60 - 100 rpmExtrusion
 100 - 200 rpm100 - 200 rpmInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow INFUSE™ 9807 Olefin Block Copolymer
RTP Company RTP 2800 B-55A HF UV Thermoplastic Polyolefin Elastomer (TEO) High Flow - UV Stabilized
RTP Company RTP 2800 B-55A HF Thermoplastic Polyolefin Elastomer (TEO) High Flow
RTP Company ESD A 2800 B-55A Black Thermoplastic Polyolefin Elastomer (TEO) ESD Protection - Static Dissipative
Avient Elastamax™ XL-2155 Thermoplastic Polyolefin Elastomer (TPO (POE))

PSTELL034 / 108257

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.