MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Atom Adhesives AA-DUCT AD1 Silver Filled Epoxy Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: AA-DUCT AD1 is a single component epoxy, formulated with pure silver power combined with organic binders and solvents to produce electrically conductive paths, films or patterns over non-conductive substrates. AA-DUCT AD1 shows slight settling when stored for a long period of time, no caking and will re disperse to a smooth homogeneous state. AA-DUCT AD1 formulation produces electrically conductive paths on a wide variety of surfaces including plastics, rubber, cloth, thermoplastic, paper, wood and many others. AA-DUCT AD1 designed for use in diversified applications as microwave EMI & RFI shielding, in the assembly or repair of printed circuit boards, wave-guides, electronic modules, flat cable, static shielding, connections, and circuitry.

Appearance: Silver

Cure Type: Heat cure

Benefits:

  • High strength
  • Perfect bond
  • EMI & RFI shielding
  • Wave guides
Substrates: Excellent choice for Integrated Circuits, aluminum, copper, magnesium, steel, bronze, nickel, Kovar, ceramic, glass, phenolic and G-10 epoxy glass boards.

Typical Application: Microwave EMI & RFI shielding, in the assembly or repair of printed circuit boards, wave-guides, electronic modules, flat cable, static shielding, connections, and circuitry.

Catalyst: Anhydride

Information provided by Atom Adhesives

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.35 g/cc2.35 g/cc
Viscosity 6800 cP6800 cPuncured
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8383
Modulus of Elasticity 4.14 GPa600 ksi
Poissons Ratio 0.350.35
Shear Strength 13.8 MPa2000 psiLap
Adhesive Bond Strength 10.3 MPa1500 psi
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 10 - 12 ohm10 - 12 ohmSheet
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.0 µm/m-°C16.7 µin/in-°F
Specific Heat Capacity 0.300 J/g-°C0.0717 BTU/lb-°F
Thermal Conductivity 41.8 W/m-K290 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 170 °C338 °F
Minimum Service Temperature, Air -45.0 °C-49.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  42.0 min
@Temperature 200 °C
0.700 hour
@Temperature 392 °F
 90.0 min
@Temperature 180 °C
1.50 hour
@Temperature 356 °F
 150 min
@Temperature 160 °C
2.50 hour
@Temperature 320 °F
Pot Life 259200 min259200 minuncured
 388800 min388800 minuncured, refrigerated
Shelf Life 6.00 Month6.00 Monthuncured
 
Component Elements PropertiesMetricEnglishComments
Silver, Ag 70 - 72 %70 - 72 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Atom Adhesives AA-DUCT 903 Epoxy Adhesive
Abatron AboCast/AboCure 8109-8
Atom Adhesives AA-SUPERTHERM 195 Epoxy Adhesive
Epoxy Technology EPO-TEK® H20E Electrically Conductive, Silver Epoxy
Sumitomo Bakelite RX® 2-501N Diallyl Phthalate Compound

PATOM041 / 172356

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.