MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type S21900 (21-6-9) Stainless Steel, sheet and strip 30% cold reduction, stress relieved at 675°C (1250°F) for 1 hour
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T S20000 Series Stainless Steel

Material Notes: Austenitic, high strength, excellent corrosion resistance, and low magnetic permeability. Applications include aircraft applications such as ducting and bellows systems, tail pipes and exhaust systems, clamps, fasteners, flanges, and hydraulic tubing.

Key Words: UNS S21900, AMS 5561, ASTM A269 (XM-10), ASTM A276 (XM-10), ASTM A314 (XM-10), ASTM A412 (XM-10), ASTM A473 (XM-10), ASTM A580 (XM-10)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.83 g/cc0.283 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 360360Converted from Rockwell C hardness.
Hardness, Knoop 392392Converted from Rockwell C hardness.
Hardness, Rockwell C 3939
Hardness, Vickers 378378Converted from Rockwell C hardness.
Tensile Strength, Ultimate 1151 MPa166900 psi
 774 MPa
@Temperature 480 °C
112000 psi
@Temperature 896 °F
Tensile Strength, Yield 1063 MPa
@Strain 0.2 %
154200 psi
@Strain 0.2 %
 774 MPa
@Strain 0.2 %,
Temperature 480 °C
112000 psi
@Strain 0.2 %,
Temperature 896 °F
Elongation at Break 18.5 %18.5 %in 50 mm
 13 %
@Temperature 480 °C
13 %
@Temperature 896 °F
in 50 mm
Modulus of Elasticity 200 GPa29000 ksiTypical for stainless steel
Machinability 30 %30 %Based on 100% machinability for AISI 1212 steel.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000730 ohm-cm0.0000730 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.7 µm/m-°C
@Temperature 25.0 - 95.0 °C
9.28 µin/in-°F
@Temperature 77.0 - 203 °F
 17.3 µm/m-°C
@Temperature 25.0 - 205 °C
9.61 µin/in-°F
@Temperature 77.0 - 401 °F
Annealed
 18.2 µm/m-°C
@Temperature 25.0 - 315 °C
10.1 µin/in-°F
@Temperature 77.0 - 599 °F
Annealed
 19.1 µm/m-°C
@Temperature 25.0 - 540 °C
10.6 µin/in-°F
@Temperature 77.0 - 1000 °F
 20.0 µm/m-°C
@Temperature 25.0 - 760 °C
11.1 µin/in-°F
@Temperature 77.0 - 1400 °F
Annealed
 20.0 µm/m-°C
@Temperature 25.0 - 870 °C
11.1 µin/in-°F
@Temperature 77.0 - 1600 °F
Annealed
 20.5 µm/m-°C
@Temperature 25.0 - 980 °C
11.4 µin/in-°F
@Temperature 77.0 - 1800 °F
Annealed
Specific Heat Capacity 0.480 J/g-°C0.115 BTU/lb-°FTypical value for stainless steel.
Thermal Conductivity  7.80 W/m-K
@Temperature -180 °C
54.1 BTU-in/hr-ft²-°F
@Temperature -292 °F
 10.9 W/m-K
@Temperature -73.0 °C
75.6 BTU-in/hr-ft²-°F
@Temperature -99.4 °F
 13.8 W/m-K
@Temperature 95.0 °C
95.8 BTU-in/hr-ft²-°F
@Temperature 203 °F
 16.1 W/m-K
@Temperature 205 °C
112 BTU-in/hr-ft²-°F
@Temperature 401 °F
 18.2 W/m-K
@Temperature 315 °C
126 BTU-in/hr-ft²-°F
@Temperature 599 °F
 20.2 W/m-K
@Temperature 425 °C
140 BTU-in/hr-ft²-°F
@Temperature 797 °F
 22.5 W/m-K
@Temperature 540 °C
156 BTU-in/hr-ft²-°F
@Temperature 1000 °F
 24.7 W/m-K
@Temperature 650 °C
171 BTU-in/hr-ft²-°F
@Temperature 1200 °F
 26.8 W/m-K
@Temperature 760 °C
186 BTU-in/hr-ft²-°F
@Temperature 1400 °F
 28.9 W/m-K
@Temperature 870 °C
201 BTU-in/hr-ft²-°F
@Temperature 1600 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 20 %20 %
Iron, Fe 64 %64 %
Manganese, Mn 9.0 %9.0 %
Nickel, Ni 6.0 %6.0 %
Nitrogen, N 0.23 %0.23 %
Phosphorus, P <= 0.060 %<= 0.060 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI E9310 Steel, normalized, machined to 13.7 mm rounds, pseudocarburized, 830°C (1525°F) reheat, 150°C (300°F) temper
AISI Type S20910 Stainless Steel, 6.4 mm diameter rod, annealed at 1120°C, 30% cold reduction
AISI E9310H Steel, normalized, machined to 25 mm (1 in.) rounds, pseudocarburized, 830°C (1525°F) reheat, 150°C (300°F) temper
AISI Type S21800 Stainless Steel, 30% cold reduction
AISI Type S21904 (Alloy 21-6-9) Stainless Steel, 30% final cold reduction

MQM22BQ / 13674

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.