Physical Properties | Metric | English | Comments |
---|
Density | 1.42 g/cc | 0.0513 lb/in³ |
Moisture Absorption at Equilibrium | 0.20 % @Temperature 23.0 °C | 0.20 % @Temperature 73.4 °F |
Water Absorption at Saturation | 1.0 % @Temperature 23.0 °C | 1.0 % @Temperature 73.4 °F |
Linear Mold Shrinkage, Flow | 0.017 cm/cm @Thickness 2.00 mm | 0.017 in/in @Thickness 0.0787 in |
Linear Mold Shrinkage, Transverse | 0.017 cm/cm @Thickness 2.00 mm | 0.017 in/in @Thickness 0.0787 in |
Melt Flow | 14 g/10 min @Load 2.16 kg, Temperature 190 °C | 14 g/10 min @Load 4.76 lb, Temperature 374 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Yield | 73.0 MPa @Temperature 23.0 °C | 10600 psi @Temperature 73.4 °F |
Tensile Stress at Strain | 0.830 MPa @Strain 0.1 %, Temperature 100 °C | 120 psi @Strain 0.1 %, Temperature 212 °F |
| 1.13 MPa @Strain 0.1 %, Temperature 80.0 °C | 164 psi @Strain 0.1 %, Temperature 176 °F |
| 2.24 MPa @Strain 0.1 %, Temperature 23.0 °C | 325 psi @Strain 0.1 %, Temperature 73.4 °F |
| 2.56 MPa @Strain 0.2 %, Temperature 100 °C | 371 psi @Strain 0.2 %, Temperature 212 °F |
| 2.80 MPa @Strain 0.1 %, Temperature -40.0 °C | 406 psi @Strain 0.1 %, Temperature -40.0 °F |
| 3.40 MPa @Strain 0.2 %, Temperature 80.0 °C | 493 psi @Strain 0.2 %, Temperature 176 °F |
| 3.83 MPa @Strain 0.3 %, Temperature 100 °C | 555 psi @Strain 0.3 %, Temperature 212 °F |
| 4.58 MPa @Strain 0.4 %, Temperature 100 °C | 664 psi @Strain 0.4 %, Temperature 212 °F |
| 5.08 MPa @Strain 0.3 %, Temperature 80.0 °C | 737 psi @Strain 0.3 %, Temperature 176 °F |
| 6.17 MPa @Strain 0.5 %, Temperature 100 °C | 895 psi @Strain 0.5 %, Temperature 212 °F |
| 6.41 MPa @Strain 0.4 %, Temperature 80.0 °C | 930 psi @Strain 0.4 %, Temperature 176 °F |
| 6.77 MPa @Strain 0.2 %, Temperature 23.0 °C | 982 psi @Strain 0.2 %, Temperature 73.4 °F |
| 7.51 MPa @Strain 0.6 %, Temperature 100 °C | 1090 psi @Strain 0.6 %, Temperature 212 °F |
| 8.21 MPa @Strain 0.7 %, Temperature 100 °C | 1190 psi @Strain 0.7 %, Temperature 212 °F |
| 8.52 MPa @Strain 0.2 %, Temperature -40.0 °C | 1240 psi @Strain 0.2 %, Temperature -40.0 °F |
| 8.53 MPa @Strain 0.5 %, Temperature 80.0 °C | 1240 psi @Strain 0.5 %, Temperature 176 °F |
| 9.28 MPa @Strain 0.8 %, Temperature 100 °C | 1350 psi @Strain 0.8 %, Temperature 212 °F |
| 9.95 MPa @Strain 0.6 %, Temperature 80.0 °C | 1440 psi @Strain 0.6 %, Temperature 176 °F |
| 10.25 MPa @Strain 0.3 %, Temperature 23.0 °C | 1487 psi @Strain 0.3 %, Temperature 73.4 °F |
| 10.25 MPa @Strain 0.9 %, Temperature 100 °C | 1487 psi @Strain 0.9 %, Temperature 212 °F |
| 10.95 MPa @Strain 1 %, Temperature 100 °C | 1588 psi @Strain 1 %, Temperature 212 °F |
| 11.4 MPa @Strain 0.7 %, Temperature 80.0 °C | 1650 psi @Strain 0.7 %, Temperature 176 °F |
| 12.07 MPa @Strain 1.1 %, Temperature 100 °C | 1751 psi @Strain 1.1 %, Temperature 212 °F |
| 12.36 MPa @Strain 0.8 %, Temperature 80.0 °C | 1793 psi @Strain 0.8 %, Temperature 176 °F |
| 12.89 MPa @Strain 0.4 %, Temperature 23.0 °C | 1870 psi @Strain 0.4 %, Temperature 73.4 °F |
| 12.92 MPa @Strain 0.3 %, Temperature -40.0 °C | 1874 psi @Strain 0.3 %, Temperature -40.0 °F |
| 13.19 MPa @Strain 1.2 %, Temperature 100 °C | 1913 psi @Strain 1.2 %, Temperature 212 °F |
| 13.59 MPa @Strain 0.9 %, Temperature 80.0 °C | 1971 psi @Strain 0.9 %, Temperature 176 °F |
| 13.98 MPa @Strain 1.3 %, Temperature 100 °C | 2028 psi @Strain 1.3 %, Temperature 212 °F |
| 14.76 MPa @Strain 1.4 %, Temperature 100 °C | 2141 psi @Strain 1.4 %, Temperature 212 °F |
| 15.17 MPa @Strain 1 %, Temperature 80.0 °C | 2200 psi @Strain 1 %, Temperature 176 °F |
| 15.61 MPa @Strain 1.5 %, Temperature 100 °C | 2264 psi @Strain 1.5 %, Temperature 212 °F |
| 16.2 MPa @Strain 0.4 %, Temperature -40.0 °C | 2350 psi @Strain 0.4 %, Temperature -40.0 °F |
| 16.27 MPa @Strain 1.1 %, Temperature 80.0 °C | 2360 psi @Strain 1.1 %, Temperature 176 °F |
| 16.33 MPa @Strain 1.6 %, Temperature 100 °C | 2368 psi @Strain 1.6 %, Temperature 212 °F |
| 17.03 MPa @Strain 1.7 %, Temperature 100 °C | 2470 psi @Strain 1.7 %, Temperature 212 °F |
| 17.34 MPa @Strain 0.5 %, Temperature 23.0 °C | 2515 psi @Strain 0.5 %, Temperature 73.4 °F |
| 17.43 MPa @Strain 1.2 %, Temperature 80.0 °C | 2528 psi @Strain 1.2 %, Temperature 176 °F |
| 17.73 MPa @Strain 1.8 %, Temperature 100 °C | 2572 psi @Strain 1.8 %, Temperature 212 °F |
| 18.37 MPa @Strain 1.9 %, Temperature 100 °C | 2664 psi @Strain 1.9 %, Temperature 212 °F |
| 18.53 MPa @Strain 1.3 %, Temperature 80.0 °C | 2688 psi @Strain 1.3 %, Temperature 176 °F |
| 19.04 MPa @Strain 2 %, Temperature 100 °C | 2762 psi @Strain 2 %, Temperature 212 °F |
| 19.49 MPa @Strain 1.4 %, Temperature 80.0 °C | 2827 psi @Strain 1.4 %, Temperature 176 °F |
| 19.68 MPa @Strain 2.1 %, Temperature 100 °C | 2854 psi @Strain 2.1 %, Temperature 212 °F |
| 20.38 MPa @Strain 2.2 %, Temperature 100 °C | 2956 psi @Strain 2.2 %, Temperature 212 °F |
| 20.53 MPa @Strain 1.5 %, Temperature 80.0 °C | 2978 psi @Strain 1.5 %, Temperature 176 °F |
| 20.85 MPa @Strain 2.3 %, Temperature 100 °C | 3024 psi @Strain 2.3 %, Temperature 212 °F |
| 21.43 MPa @Strain 2.4 %, Temperature 100 °C | 3108 psi @Strain 2.4 %, Temperature 212 °F |
| 21.44 MPa @Strain 0.5 %, Temperature -40.0 °C | 3110 psi @Strain 0.5 %, Temperature -40.0 °F |
| 21.46 MPa @Strain 1.6 %, Temperature 80.0 °C | 3113 psi @Strain 1.6 %, Temperature 176 °F |
| 21.95 MPa @Strain 2.5 %, Temperature 100 °C | 3184 psi @Strain 2.5 %, Temperature 212 °F |
| 22.39 MPa @Strain 1.7 %, Temperature 80.0 °C | 3247 psi @Strain 1.7 %, Temperature 176 °F |
| 22.48 MPa @Strain 2.6 %, Temperature 100 °C | 3260 psi @Strain 2.6 %, Temperature 212 °F |
| 22.54 MPa @Strain 0.6 %, Temperature 23.0 °C | 3269 psi @Strain 0.6 %, Temperature 73.4 °F |
| 23.06 MPa @Strain 2.7 %, Temperature 100 °C | 3345 psi @Strain 2.7 %, Temperature 212 °F |
| 23.26 MPa @Strain 1.8 %, Temperature 80.0 °C | 3374 psi @Strain 1.8 %, Temperature 176 °F |
| 23.47 MPa @Strain 2.8 %, Temperature 100 °C | 3404 psi @Strain 2.8 %, Temperature 212 °F |
| 23.76 MPa @Strain 2.9 %, Temperature 100 °C | 3446 psi @Strain 2.9 %, Temperature 212 °F |
| 24.07 MPa @Strain 1.9 %, Temperature 80.0 °C | 3491 psi @Strain 1.9 %, Temperature 176 °F |
| 24.11 MPa @Strain 3 %, Temperature 100 °C | 3497 psi @Strain 3 %, Temperature 212 °F |
| 24.61 MPa @Strain 50 %, Temperature 100 °C | 3569 psi @Strain 50 %, Temperature 212 °F |
| 24.7 MPa @Strain 49 %, Temperature 100 °C | 3580 psi @Strain 49 %, Temperature 212 °F |
| 24.75 MPa @Strain 48 %, Temperature 100 °C | 3590 psi @Strain 48 %, Temperature 212 °F |
| 24.81 MPa @Strain 3.1 %, Temperature 100 °C | 3598 psi @Strain 3.1 %, Temperature 212 °F |
| 24.83 MPa @Strain 47 %, Temperature 100 °C | 3601 psi @Strain 47 %, Temperature 212 °F |
| 24.88 MPa @Strain 2 %, Temperature 80.0 °C | 3609 psi @Strain 2 %, Temperature 176 °F |
| 24.92 MPa @Strain 46 %, Temperature 100 °C | 3614 psi @Strain 46 %, Temperature 212 °F |
| 24.94 MPa @Strain 45 %, Temperature 100 °C | 3617 psi @Strain 45 %, Temperature 212 °F |
| 25.07 MPa @Strain 44 %, Temperature 100 °C | 3636 psi @Strain 44 %, Temperature 212 °F |
| 25.16 MPa @Strain 43 %, Temperature 100 °C | 3649 psi @Strain 43 %, Temperature 212 °F |
| 25.16 MPa @Strain 3.2 %, Temperature 100 °C | 3649 psi @Strain 3.2 %, Temperature 212 °F |
| 25.23 MPa @Strain 42 %, Temperature 100 °C | 3659 psi @Strain 42 %, Temperature 212 °F |
| 25.26 MPa @Strain 0.6 %, Temperature -40.0 °C | 3664 psi @Strain 0.6 %, Temperature -40.0 °F |
| 25.29 MPa @Strain 41 %, Temperature 100 °C | 3668 psi @Strain 41 %, Temperature 212 °F |
| 25.39 MPa @Strain 40 %, Temperature 100 °C | 3683 psi @Strain 40 %, Temperature 212 °F |
| 25.5 MPa @Strain 39 %, Temperature 100 °C | 3700 psi @Strain 39 %, Temperature 212 °F |
| 25.51 MPa @Strain 3.3 %, Temperature 100 °C | 3700 psi @Strain 3.3 %, Temperature 212 °F |
| 25.55 MPa @Strain 38 %, Temperature 100 °C | 3706 psi @Strain 38 %, Temperature 212 °F |
| 25.64 MPa @Strain 2.1 %, Temperature 80.0 °C | 3719 psi @Strain 2.1 %, Temperature 176 °F |
| 25.67 MPa @Strain 37 %, Temperature 100 °C | 3723 psi @Strain 37 %, Temperature 212 °F |
| 25.78 MPa @Strain 36 %, Temperature 100 °C | 3739 psi @Strain 36 %, Temperature 212 °F |
| 25.86 MPa @Strain 35 %, Temperature 100 °C | 3751 psi @Strain 35 %, Temperature 212 °F |
| 25.97 MPa @Strain 3.4 %, Temperature 100 °C | 3767 psi @Strain 3.4 %, Temperature 212 °F |
| 25.98 MPa @Strain 34 %, Temperature 100 °C | 3768 psi @Strain 34 %, Temperature 212 °F |
| 26.09 MPa @Strain 33 %, Temperature 100 °C | 3784 psi @Strain 33 %, Temperature 212 °F |
| 26.19 MPa @Strain 32 %, Temperature 100 °C | 3799 psi @Strain 32 %, Temperature 212 °F |
| 26.21 MPa @Strain 3.5 %, Temperature 100 °C | 3801 psi @Strain 3.5 %, Temperature 212 °F |
| 26.31 MPa @Strain 31 %, Temperature 100 °C | 3816 psi @Strain 31 %, Temperature 212 °F |
| 26.39 MPa @Strain 2.2 %, Temperature 80.0 °C | 3828 psi @Strain 2.2 %, Temperature 176 °F |
| 26.41 MPa @Strain 30 %, Temperature 100 °C | 3830 psi @Strain 30 %, Temperature 212 °F |
| 26.44 MPa @Strain 3.6 %, Temperature 100 °C | 3835 psi @Strain 3.6 %, Temperature 212 °F |
| 26.56 MPa @Strain 29 %, Temperature 100 °C | 3852 psi @Strain 29 %, Temperature 212 °F |
| 26.67 MPa @Strain 3.7 %, Temperature 100 °C | 3868 psi @Strain 3.7 %, Temperature 212 °F |
| 26.68 MPa @Strain 28 %, Temperature 100 °C | 3870 psi @Strain 28 %, Temperature 212 °F |
| 26.88 MPa @Strain 27 %, Temperature 100 °C | 3899 psi @Strain 27 %, Temperature 212 °F |
| 26.88 MPa @Strain 0.7 %, Temperature 23.0 °C | 3899 psi @Strain 0.7 %, Temperature 73.4 °F |
| 26.98 MPa @Strain 26 %, Temperature 100 °C | 3913 psi @Strain 26 %, Temperature 212 °F |
| 27.08 MPa @Strain 3.8 %, Temperature 100 °C | 3928 psi @Strain 3.8 %, Temperature 212 °F |
| 27.15 MPa @Strain 2.3 %, Temperature 80.0 °C | 3938 psi @Strain 2.3 %, Temperature 176 °F |
| 27.16 MPa @Strain 25 %, Temperature 100 °C | 3939 psi @Strain 25 %, Temperature 212 °F |
| 27.31 MPa @Strain 3.9 %, Temperature 100 °C | 3961 psi @Strain 3.9 %, Temperature 212 °F |
| 27.32 MPa @Strain 24 %, Temperature 100 °C | 3962 psi @Strain 24 %, Temperature 212 °F |
| 27.5 MPa @Strain 23 %, Temperature 100 °C | 3990 psi @Strain 23 %, Temperature 212 °F |
| 27.54 MPa @Strain 4 %, Temperature 100 °C | 3994 psi @Strain 4 %, Temperature 212 °F |
| 27.67 MPa @Strain 22 %, Temperature 100 °C | 4013 psi @Strain 22 %, Temperature 212 °F |
| 27.72 MPa @Strain 4.1 %, Temperature 100 °C | 4020 psi @Strain 4.1 %, Temperature 212 °F |
| 27.78 MPa @Strain 2.4 %, Temperature 80.0 °C | 4029 psi @Strain 2.4 %, Temperature 176 °F |
| 27.85 MPa @Strain 21 %, Temperature 100 °C | 4039 psi @Strain 21 %, Temperature 212 °F |
| 27.89 MPa @Strain 4.2 %, Temperature 100 °C | 4045 psi @Strain 4.2 %, Temperature 212 °F |
| 28.06 MPa @Strain 20 %, Temperature 100 °C | 4070 psi @Strain 20 %, Temperature 212 °F |
| 28.13 MPa @Strain 4.3 %, Temperature 100 °C | 4080 psi @Strain 4.3 %, Temperature 212 °F |
| 28.16 MPa @Strain 0.7 %, Temperature -40.0 °C | 4084 psi @Strain 0.7 %, Temperature -40.0 °F |
| 28.22 MPa @Strain 19 %, Temperature 100 °C | 4093 psi @Strain 19 %, Temperature 212 °F |
| 28.3 MPa @Strain 4.4 %, Temperature 100 °C | 4100 psi @Strain 4.4 %, Temperature 212 °F |
| 28.5 MPa @Strain 18 %, Temperature 100 °C | 4130 psi @Strain 18 %, Temperature 212 °F |
| 28.53 MPa @Strain 4.5 %, Temperature 100 °C | 4138 psi @Strain 4.5 %, Temperature 212 °F |
| 28.54 MPa @Strain 2.5 %, Temperature 80.0 °C | 4139 psi @Strain 2.5 %, Temperature 176 °F |
| 28.65 MPa @Strain 4.6 %, Temperature 100 °C | 4155 psi @Strain 4.6 %, Temperature 212 °F |
| 28.71 MPa @Strain 17 %, Temperature 100 °C | 4164 psi @Strain 17 %, Temperature 212 °F |
| 28.88 MPa @Strain 4.7 %, Temperature 100 °C | 4189 psi @Strain 4.7 %, Temperature 212 °F |
| 28.92 MPa @Strain 16 %, Temperature 100 °C | 4194 psi @Strain 16 %, Temperature 212 °F |
| 29.06 MPa @Strain 4.8 %, Temperature 100 °C | 4215 psi @Strain 4.8 %, Temperature 212 °F |
| 29.09 MPa @Strain 0.8 %, Temperature 23.0 °C | 4219 psi @Strain 0.8 %, Temperature 73.4 °F |
| 29.18 MPa @Strain 2.6 %, Temperature 80.0 °C | 4232 psi @Strain 2.6 %, Temperature 176 °F |
| 29.18 MPa @Strain 4.9 %, Temperature 100 °C | 4232 psi @Strain 4.9 %, Temperature 212 °F |
| 29.23 MPa @Strain 5.0 %, Temperature 100 °C | 4239 psi @Strain 5.0 %, Temperature 212 °F |
| 29.23 MPa @Strain 15 %, Temperature 100 °C | 4239 psi @Strain 15 %, Temperature 212 °F |
| 29.44 MPa @Strain 14 %, Temperature 100 °C | 4270 psi @Strain 14 %, Temperature 212 °F |
| 29.68 MPa @Strain 13 %, Temperature 100 °C | 4305 psi @Strain 13 %, Temperature 212 °F |
| 29.68 MPa @Strain 5.5 %, Temperature 100 °C | 4305 psi @Strain 5.5 %, Temperature 212 °F |
| 29.87 MPa @Strain 2.7 %, Temperature 80.0 °C | 4332 psi @Strain 2.7 %, Temperature 176 °F |
| 29.93 MPa @Strain 12 %, Temperature 100 °C | 4341 psi @Strain 12 %, Temperature 212 °F |
| 30.15 MPa @Strain 6.0 %, Temperature 100 °C | 4373 psi @Strain 6.0 %, Temperature 212 °F |
| 30.23 MPa @Strain 11 %, Temperature 100 °C | 4384 psi @Strain 11 %, Temperature 212 °F |
| 30.38 MPa @Strain 6.5 %, Temperature 100 °C | 4406 psi @Strain 6.5 %, Temperature 212 °F |
| 30.39 MPa @Strain 2.8 %, Temperature 80.0 °C | 4408 psi @Strain 2.8 %, Temperature 176 °F |
| 30.48 MPa @Strain 9.5 %, Temperature 100 °C | 4421 psi @Strain 9.5 %, Temperature 212 °F |
| 30.48 MPa @Strain 10 %, Temperature 100 °C | 4421 psi @Strain 10 %, Temperature 212 °F |
| 30.5 MPa @Strain 7.0 %, Temperature 100 °C | 4420 psi @Strain 7.0 %, Temperature 212 °F |
| 30.54 MPa @Strain 9.0 %, Temperature 100 °C | 4429 psi @Strain 9.0 %, Temperature 212 °F |
| 30.59 MPa @Strain 7.5 %, Temperature 100 °C | 4437 psi @Strain 7.5 %, Temperature 212 °F |
| 30.59 MPa @Strain 8.5 %, Temperature 100 °C | 4437 psi @Strain 8.5 %, Temperature 212 °F |
| 30.6 MPa @Strain 8.0 %, Temperature 100 °C | 4440 psi @Strain 8.0 %, Temperature 212 °F |
| 31.03 MPa @Strain 2.9 %, Temperature 80.0 °C | 4501 psi @Strain 2.9 %, Temperature 176 °F |
| 31.18 MPa @Strain 0.9 %, Temperature 23.0 °C | 4522 psi @Strain 0.9 %, Temperature 73.4 °F |
| 31.61 MPa @Strain 3 %, Temperature 80.0 °C | 4585 psi @Strain 3 %, Temperature 176 °F |
| 31.7 MPa @Strain 0.8 %, Temperature -40.0 °C | 4600 psi @Strain 0.8 %, Temperature -40.0 °F |
| 31.96 MPa @Strain 3.1 %, Temperature 80.0 °C | 4635 psi @Strain 3.1 %, Temperature 176 °F |
| 32.46 MPa @Strain 3.2 %, Temperature 80.0 °C | 4708 psi @Strain 3.2 %, Temperature 176 °F |
| 32.89 MPa @Strain 3.3 %, Temperature 80.0 °C | 4770 psi @Strain 3.3 %, Temperature 176 °F |
| 33.35 MPa @Strain 3.4 %, Temperature 80.0 °C | 4837 psi @Strain 3.4 %, Temperature 176 °F |
| 33.5 MPa @Strain 1 %, Temperature 23.0 °C | 4860 psi @Strain 1 %, Temperature 73.4 °F |
| 33.76 MPa @Strain 3.5 %, Temperature 80.0 °C | 4896 psi @Strain 3.5 %, Temperature 176 °F |
| 34.11 MPa @Strain 49 %, Temperature 80.0 °C | 4947 psi @Strain 49 %, Temperature 176 °F |
| 34.11 MPa @Strain 50 %, Temperature 80.0 °C | 4947 psi @Strain 50 %, Temperature 176 °F |
| 34.22 MPa @Strain 3.6 %, Temperature 80.0 °C | 4963 psi @Strain 3.6 %, Temperature 176 °F |
| 34.27 MPa @Strain 48 %, Temperature 80.0 °C | 4970 psi @Strain 48 %, Temperature 176 °F |
| 34.37 MPa @Strain 47 %, Temperature 80.0 °C | 4985 psi @Strain 47 %, Temperature 176 °F |
| 34.38 MPa @Strain 46 %, Temperature 80.0 °C | 4986 psi @Strain 46 %, Temperature 176 °F |
| 34.53 MPa @Strain 45 %, Temperature 80.0 °C | 5008 psi @Strain 45 %, Temperature 176 °F |
| 34.61 MPa @Strain 44 %, Temperature 80.0 °C | 5020 psi @Strain 44 %, Temperature 176 °F |
| 34.63 MPa @Strain 3.7 %, Temperature 80.0 °C | 5023 psi @Strain 3.7 %, Temperature 176 °F |
| 34.73 MPa @Strain 43 %, Temperature 80.0 °C | 5037 psi @Strain 43 %, Temperature 176 °F |
| 34.79 MPa @Strain 42 %, Temperature 80.0 °C | 5046 psi @Strain 42 %, Temperature 176 °F |
| 34.9 MPa @Strain 41 %, Temperature 80.0 °C | 5060 psi @Strain 41 %, Temperature 176 °F |
| 34.98 MPa @Strain 3.8 %, Temperature 80.0 °C | 5073 psi @Strain 3.8 %, Temperature 176 °F |
| 35.03 MPa @Strain 40 %, Temperature 80.0 °C | 5081 psi @Strain 40 %, Temperature 176 °F |
| 35.16 MPa @Strain 39 %, Temperature 80.0 °C | 5100 psi @Strain 39 %, Temperature 176 °F |
| 35.26 MPa @Strain 38 %, Temperature 80.0 °C | 5114 psi @Strain 38 %, Temperature 176 °F |
| 35.41 MPa @Strain 37 %, Temperature 80.0 °C | 5136 psi @Strain 37 %, Temperature 176 °F |
| 35.44 MPa @Strain 3.9 %, Temperature 80.0 °C | 5140 psi @Strain 3.9 %, Temperature 176 °F |
| 35.53 MPa @Strain 0.9 %, Temperature -40.0 °C | 5153 psi @Strain 0.9 %, Temperature -40.0 °F |
| 35.54 MPa @Strain 36 %, Temperature 80.0 °C | 5155 psi @Strain 36 %, Temperature 176 °F |
| 35.63 MPa @Strain 35 %, Temperature 80.0 °C | 5168 psi @Strain 35 %, Temperature 176 °F |
| 35.67 MPa @Strain 4 %, Temperature 80.0 °C | 5174 psi @Strain 4 %, Temperature 176 °F |
| 35.76 MPa @Strain 34 %, Temperature 80.0 °C | 5187 psi @Strain 34 %, Temperature 176 °F |
| 35.83 MPa @Strain 1.1 %, Temperature 23.0 °C | 5197 psi @Strain 1.1 %, Temperature 73.4 °F |
| 35.85 MPa @Strain 4.1 %, Temperature 80.0 °C | 5200 psi @Strain 4.1 %, Temperature 176 °F |
| 35.93 MPa @Strain 33 %, Temperature 80.0 °C | 5211 psi @Strain 33 %, Temperature 176 °F |
| 36.04 MPa @Strain 32 %, Temperature 80.0 °C | 5227 psi @Strain 32 %, Temperature 176 °F |
| 36.19 MPa @Strain 31 %, Temperature 80.0 °C | 5249 psi @Strain 31 %, Temperature 176 °F |
| 36.25 MPa @Strain 4.2 %, Temperature 80.0 °C | 5258 psi @Strain 4.2 %, Temperature 176 °F |
| 36.33 MPa @Strain 30 %, Temperature 80.0 °C | 5269 psi @Strain 30 %, Temperature 176 °F |
| 36.49 MPa @Strain 29 %, Temperature 80.0 °C | 5292 psi @Strain 29 %, Temperature 176 °F |
| 36.54 MPa @Strain 4.3 %, Temperature 80.0 °C | 5300 psi @Strain 4.3 %, Temperature 176 °F |
| 36.62 MPa @Strain 28 %, Temperature 80.0 °C | 5311 psi @Strain 28 %, Temperature 176 °F |
| 36.8 MPa @Strain 27 %, Temperature 80.0 °C | 5340 psi @Strain 27 %, Temperature 176 °F |
| 36.83 MPa @Strain 4.4 %, Temperature 80.0 °C | 5342 psi @Strain 4.4 %, Temperature 176 °F |
| 36.99 MPa @Strain 26 %, Temperature 80.0 °C | 5365 psi @Strain 26 %, Temperature 176 °F |
| 37.01 MPa @Strain 4.5 %, Temperature 80.0 °C | 5368 psi @Strain 4.5 %, Temperature 176 °F |
| 37.16 MPa @Strain 25 %, Temperature 80.0 °C | 5390 psi @Strain 25 %, Temperature 176 °F |
| 37.24 MPa @Strain 4.6 %, Temperature 80.0 °C | 5401 psi @Strain 4.6 %, Temperature 176 °F |
| 37.3 MPa @Strain 24 %, Temperature 80.0 °C | 5410 psi @Strain 24 %, Temperature 176 °F |
| 37.41 MPa @Strain 4.7 %, Temperature 80.0 °C | 5426 psi @Strain 4.7 %, Temperature 176 °F |
| 37.55 MPa @Strain 23 %, Temperature 80.0 °C | 5446 psi @Strain 23 %, Temperature 176 °F |
| 37.65 MPa @Strain 4.8 %, Temperature 80.0 °C | 5461 psi @Strain 4.8 %, Temperature 176 °F |
| 37.73 MPa @Strain 22 %, Temperature 80.0 °C | 5472 psi @Strain 22 %, Temperature 176 °F |
| 37.8 MPa @Strain 1.2 %, Temperature 23.0 °C | 5480 psi @Strain 1.2 %, Temperature 73.4 °F |
| 37.82 MPa @Strain 4.9 %, Temperature 80.0 °C | 5485 psi @Strain 4.9 %, Temperature 176 °F |
| 37.94 MPa @Strain 21 %, Temperature 80.0 °C | 5503 psi @Strain 21 %, Temperature 176 °F |
| 38.05 MPa @Strain 5.0 %, Temperature 80.0 °C | 5519 psi @Strain 5.0 %, Temperature 176 °F |
| 38.16 MPa @Strain 20 %, Temperature 80.0 °C | 5535 psi @Strain 20 %, Temperature 176 °F |
| 38.33 MPa @Strain 19 %, Temperature 80.0 °C | 5559 psi @Strain 19 %, Temperature 176 °F |
| 38.44 MPa @Strain 1 %, Temperature -40.0 °C | 5575 psi @Strain 1 %, Temperature -40.0 °F |
| 38.57 MPa @Strain 18 %, Temperature 80.0 °C | 5594 psi @Strain 18 %, Temperature 176 °F |
| 38.57 MPa @Strain 5.5 %, Temperature 80.0 °C | 5594 psi @Strain 5.5 %, Temperature 176 °F |
| 38.8 MPa @Strain 17 %, Temperature 80.0 °C | 5630 psi @Strain 17 %, Temperature 176 °F |
| 39.02 MPa @Strain 16 %, Temperature 80.0 °C | 5659 psi @Strain 16 %, Temperature 176 °F |
| 39.23 MPa @Strain 6.0 %, Temperature 80.0 °C | 5690 psi @Strain 6.0 %, Temperature 176 °F |
| 39.27 MPa @Strain 15 %, Temperature 80.0 °C | 5696 psi @Strain 15 %, Temperature 176 °F |
| 39.46 MPa @Strain 14 %, Temperature 80.0 °C | 5723 psi @Strain 14 %, Temperature 176 °F |
| 39.63 MPa @Strain 6.5 %, Temperature 80.0 °C | 5748 psi @Strain 6.5 %, Temperature 176 °F |
| 39.66 MPa @Strain 1.3 %, Temperature 23.0 °C | 5752 psi @Strain 1.3 %, Temperature 73.4 °F |
| 39.75 MPa @Strain 13 %, Temperature 80.0 °C | 5765 psi @Strain 13 %, Temperature 176 °F |
| 39.92 MPa @Strain 12 %, Temperature 80.0 °C | 5790 psi @Strain 12 %, Temperature 176 °F |
| 39.92 MPa @Strain 7.0 %, Temperature 80.0 °C | 5790 psi @Strain 7.0 %, Temperature 176 °F |
| 40.11 MPa @Strain 7.5 %, Temperature 80.0 °C | 5817 psi @Strain 7.5 %, Temperature 176 °F |
| 40.13 MPa @Strain 11 %, Temperature 80.0 °C | 5820 psi @Strain 11 %, Temperature 176 °F |
| 40.21 MPa @Strain 10 %, Temperature 80.0 °C | 5832 psi @Strain 10 %, Temperature 176 °F |
| 40.23 MPa @Strain 8.0 %, Temperature 80.0 °C | 5835 psi @Strain 8.0 %, Temperature 176 °F |
| 40.3 MPa @Strain 8.5 %, Temperature 80.0 °C | 5850 psi @Strain 8.5 %, Temperature 176 °F |
| 40.31 MPa @Strain 9.5 %, Temperature 80.0 °C | 5846 psi @Strain 9.5 %, Temperature 176 °F |
| 40.33 MPa @Strain 9.0 %, Temperature 80.0 °C | 5849 psi @Strain 9.0 %, Temperature 176 °F |
| 41.17 MPa @Strain 1.4 %, Temperature 23.0 °C | 5971 psi @Strain 1.4 %, Temperature 73.4 °F |
| 41.26 MPa @Strain 1.1 %, Temperature -40.0 °C | 5984 psi @Strain 1.1 %, Temperature -40.0 °F |
| 42.79 MPa @Strain 1.5 %, Temperature 23.0 °C | 6206 psi @Strain 1.5 %, Temperature 73.4 °F |
| 44.42 MPa @Strain 1.6 %, Temperature 23.0 °C | 6443 psi @Strain 1.6 %, Temperature 73.4 °F |
| 44.82 MPa @Strain 1.2 %, Temperature -40.0 °C | 6501 psi @Strain 1.2 %, Temperature -40.0 °F |
| 45.64 MPa @Strain 1.7 %, Temperature 23.0 °C | 6620 psi @Strain 1.7 %, Temperature 73.4 °F |
| 46.68 MPa @Strain 1.8 %, Temperature 23.0 °C | 6770 psi @Strain 1.8 %, Temperature 73.4 °F |
| 48.15 MPa @Strain 1.3 %, Temperature -40.0 °C | 6984 psi @Strain 1.3 %, Temperature -40.0 °F |
| 48.17 MPa @Strain 1.9 %, Temperature 23.0 °C | 6986 psi @Strain 1.9 %, Temperature 73.4 °F |
| 49.47 MPa @Strain 2 %, Temperature 23.0 °C | 7175 psi @Strain 2 %, Temperature 73.4 °F |
| 50.46 MPa @Strain 2.1 %, Temperature 23.0 °C | 7319 psi @Strain 2.1 %, Temperature 73.4 °F |
| 50.69 MPa @Strain 1.4 %, Temperature -40.0 °C | 7352 psi @Strain 1.4 %, Temperature -40.0 °F |
| 51.56 MPa @Strain 2.2 %, Temperature 23.0 °C | 7478 psi @Strain 2.2 %, Temperature 73.4 °F |
| 52.49 MPa @Strain 2.3 %, Temperature 23.0 °C | 7613 psi @Strain 2.3 %, Temperature 73.4 °F |
| 53.15 MPa @Strain 1.5 %, Temperature -40.0 °C | 7709 psi @Strain 1.5 %, Temperature -40.0 °F |
| 53.42 MPa @Strain 2.4 %, Temperature 23.0 °C | 7748 psi @Strain 2.4 %, Temperature 73.4 °F |
| 54.41 MPa @Strain 2.5 %, Temperature 23.0 °C | 7892 psi @Strain 2.5 %, Temperature 73.4 °F |
| 55.1 MPa @Strain 2.6 %, Temperature 23.0 °C | 7990 psi @Strain 2.6 %, Temperature 73.4 °F |
| 55.97 MPa @Strain 2.7 %, Temperature 23.0 °C | 8118 psi @Strain 2.7 %, Temperature 73.4 °F |
| 56.01 MPa @Strain 1.6 %, Temperature -40.0 °C | 8124 psi @Strain 1.6 %, Temperature -40.0 °F |
| 56.73 MPa @Strain 2.8 %, Temperature 23.0 °C | 8228 psi @Strain 2.8 %, Temperature 73.4 °F |
| 57.6 MPa @Strain 2.9 %, Temperature 23.0 °C | 8350 psi @Strain 2.9 %, Temperature 73.4 °F |
| 58.24 MPa @Strain 3 %, Temperature 23.0 °C | 8447 psi @Strain 3 %, Temperature 73.4 °F |
| 58.24 MPa @Strain 1.7 %, Temperature -40.0 °C | 8447 psi @Strain 1.7 %, Temperature -40.0 °F |
| 58.82 MPa @Strain 3.1 %, Temperature 23.0 °C | 8531 psi @Strain 3.1 %, Temperature 73.4 °F |
| 59.22 MPa @Strain 3.2 %, Temperature 23.0 °C | 8589 psi @Strain 3.2 %, Temperature 73.4 °F |
| 59.81 MPa @Strain 3.3 %, Temperature 23.0 °C | 8675 psi @Strain 3.3 %, Temperature 73.4 °F |
| 60.5 MPa @Strain 3.4 %, Temperature 23.0 °C | 8770 psi @Strain 3.4 %, Temperature 73.4 °F |
| 60.5 MPa @Strain 1.8 %, Temperature -40.0 °C | 8770 psi @Strain 1.8 %, Temperature -40.0 °F |
| 60.97 MPa @Strain 3.5 %, Temperature 23.0 °C | 8843 psi @Strain 3.5 %, Temperature 73.4 °F |
| 61.49 MPa @Strain 3.6 %, Temperature 23.0 °C | 8918 psi @Strain 3.6 %, Temperature 73.4 °F |
| 61.84 MPa @Strain 3.7 %, Temperature 23.0 °C | 8969 psi @Strain 3.7 %, Temperature 73.4 °F |
| 62.3 MPa @Strain 3.8 %, Temperature 23.0 °C | 9040 psi @Strain 3.8 %, Temperature 73.4 °F |
| 62.65 MPa @Strain 3.9 %, Temperature 23.0 °C | 9087 psi @Strain 3.9 %, Temperature 73.4 °F |
| 62.71 MPa @Strain 1.9 %, Temperature -40.0 °C | 9095 psi @Strain 1.9 %, Temperature -40.0 °F |
| 63.0 MPa @Strain 4 %, Temperature 23.0 °C | 9140 psi @Strain 4 %, Temperature 73.4 °F |
| 63.35 MPa @Strain 4.1 %, Temperature 23.0 °C | 9188 psi @Strain 4.1 %, Temperature 73.4 °F |
| 63.81 MPa @Strain 4.2 %, Temperature 23.0 °C | 9255 psi @Strain 4.2 %, Temperature 73.4 °F |
| 63.99 MPa @Strain 4.3 %, Temperature 23.0 °C | 9281 psi @Strain 4.3 %, Temperature 73.4 °F |
| 64.16 MPa @Strain 4.4 %, Temperature 23.0 °C | 9306 psi @Strain 4.4 %, Temperature 73.4 °F |
| 64.45 MPa @Strain 2 %, Temperature -40.0 °C | 9348 psi @Strain 2 %, Temperature -40.0 °F |
| 64.51 MPa @Strain 4.5 %, Temperature 23.0 °C | 9356 psi @Strain 4.5 %, Temperature 73.4 °F |
| 64.86 MPa @Strain 4.6 %, Temperature 23.0 °C | 9407 psi @Strain 4.6 %, Temperature 73.4 °F |
| 65.09 MPa @Strain 4.7 %, Temperature 23.0 °C | 9441 psi @Strain 4.7 %, Temperature 73.4 °F |
| 65.32 MPa @Strain 4.8 %, Temperature 23.0 °C | 9474 psi @Strain 4.8 %, Temperature 73.4 °F |
| 65.44 MPa @Strain 4.9 %, Temperature 23.0 °C | 9491 psi @Strain 4.9 %, Temperature 73.4 °F |
| 65.48 MPa @Strain 31 %, Temperature 23.0 °C | 9497 psi @Strain 31 %, Temperature 73.4 °F |
| 65.52 MPa @Strain 30 %, Temperature 23.0 °C | 9503 psi @Strain 30 %, Temperature 73.4 °F |
| 65.7 MPa @Strain 29 %, Temperature 23.0 °C | 9530 psi @Strain 29 %, Temperature 73.4 °F |
| 65.73 MPa @Strain 5.0 %, Temperature 23.0 °C | 9533 psi @Strain 5.0 %, Temperature 73.4 °F |
| 65.88 MPa @Strain 28 %, Temperature 23.0 °C | 9555 psi @Strain 28 %, Temperature 73.4 °F |
| 65.95 MPa @Strain 27 %, Temperature 23.0 °C | 9565 psi @Strain 27 %, Temperature 73.4 °F |
| 66.08 MPa @Strain 26 %, Temperature 23.0 °C | 9584 psi @Strain 26 %, Temperature 73.4 °F |
| 66.13 MPa @Strain 2.1 %, Temperature -40.0 °C | 9591 psi @Strain 2.1 %, Temperature -40.0 °F |
| 66.26 MPa @Strain 25 %, Temperature 23.0 °C | 9610 psi @Strain 25 %, Temperature 73.4 °F |
| 66.27 MPa @Strain 5.5 %, Temperature 23.0 °C | 9612 psi @Strain 5.5 %, Temperature 73.4 °F |
| 66.42 MPa @Strain 24 %, Temperature 23.0 °C | 9633 psi @Strain 24 %, Temperature 73.4 °F |
| 66.55 MPa @Strain 23 %, Temperature 23.0 °C | 9652 psi @Strain 23 %, Temperature 73.4 °F |
| 66.64 MPa @Strain 22 %, Temperature 23.0 °C | 9665 psi @Strain 22 %, Temperature 73.4 °F |
| 66.82 MPa @Strain 21 %, Temperature 23.0 °C | 9691 psi @Strain 21 %, Temperature 73.4 °F |
| 66.94 MPa @Strain 20 %, Temperature 23.0 °C | 9709 psi @Strain 20 %, Temperature 73.4 °F |
| 66.98 MPa @Strain 6.0 %, Temperature 23.0 °C | 9715 psi @Strain 6.0 %, Temperature 73.4 °F |
| 67.13 MPa @Strain 19 %, Temperature 23.0 °C | 9736 psi @Strain 19 %, Temperature 73.4 °F |
| 67.29 MPa @Strain 18 %, Temperature 23.0 °C | 9760 psi @Strain 18 %, Temperature 73.4 °F |
| 67.41 MPa @Strain 6.5 %, Temperature 23.0 °C | 9777 psi @Strain 6.5 %, Temperature 73.4 °F |
| 67.45 MPa @Strain 17 %, Temperature 23.0 °C | 9783 psi @Strain 17 %, Temperature 73.4 °F |
| 67.6 MPa @Strain 16 %, Temperature 23.0 °C | 9800 psi @Strain 16 %, Temperature 73.4 °F |
| 67.74 MPa @Strain 7.0 %, Temperature 23.0 °C | 9825 psi @Strain 7.0 %, Temperature 73.4 °F |
| 67.79 MPa @Strain 15 %, Temperature 23.0 °C | 9832 psi @Strain 15 %, Temperature 73.4 °F |
| 67.93 MPa @Strain 7.5 %, Temperature 23.0 °C | 9852 psi @Strain 7.5 %, Temperature 73.4 °F |
| 67.93 MPa @Strain 2.2 %, Temperature -40.0 °C | 9852 psi @Strain 2.2 %, Temperature -40.0 °F |
| 67.95 MPa @Strain 14 %, Temperature 23.0 °C | 9855 psi @Strain 14 %, Temperature 73.4 °F |
| 68.07 MPa @Strain 13 %, Temperature 23.0 °C | 9873 psi @Strain 13 %, Temperature 73.4 °F |
| 68.12 MPa @Strain 8.0 %, Temperature 23.0 °C | 9880 psi @Strain 8.0 %, Temperature 73.4 °F |
| 68.21 MPa @Strain 12 %, Temperature 23.0 °C | 9893 psi @Strain 12 %, Temperature 73.4 °F |
| 68.24 MPa @Strain 8.5 %, Temperature 23.0 °C | 9897 psi @Strain 8.5 %, Temperature 73.4 °F |
| 68.28 MPa @Strain 11 %, Temperature 23.0 °C | 9903 psi @Strain 11 %, Temperature 73.4 °F |
| 68.29 MPa @Strain 9.0 %, Temperature 23.0 °C | 9905 psi @Strain 9.0 %, Temperature 73.4 °F |
| 68.32 MPa @Strain 9.5 %, Temperature 23.0 °C | 9909 psi @Strain 9.5 %, Temperature 73.4 °F |
| 68.34 MPa @Strain 10 %, Temperature 23.0 °C | 9912 psi @Strain 10 %, Temperature 73.4 °F |
| 69.91 MPa @Strain 2.3 %, Temperature -40.0 °C | 10140 psi @Strain 2.3 %, Temperature -40.0 °F |
| 71.94 MPa @Strain 2.4 %, Temperature -40.0 °C | 10430 psi @Strain 2.4 %, Temperature -40.0 °F |
| 73.39 MPa @Strain 2.5 %, Temperature -40.0 °C | 10640 psi @Strain 2.5 %, Temperature -40.0 °F |
| 74.9 MPa @Strain 2.6 %, Temperature -40.0 °C | 10900 psi @Strain 2.6 %, Temperature -40.0 °F |
| 76.24 MPa @Strain 2.7 %, Temperature -40.0 °C | 11060 psi @Strain 2.7 %, Temperature -40.0 °F |
| 77.75 MPa @Strain 2.8 %, Temperature -40.0 °C | 11280 psi @Strain 2.8 %, Temperature -40.0 °F |
| 78.85 MPa @Strain 2.9 %, Temperature -40.0 °C | 11440 psi @Strain 2.9 %, Temperature -40.0 °F |
| 80.01 MPa @Strain 3 %, Temperature -40.0 °C | 11600 psi @Strain 3 %, Temperature -40.0 °F |
| 81.35 MPa @Strain 3.1 %, Temperature -40.0 °C | 11800 psi @Strain 3.1 %, Temperature -40.0 °F |
| 82.39 MPa @Strain 3.2 %, Temperature -40.0 °C | 11950 psi @Strain 3.2 %, Temperature -40.0 °F |
| 83.03 MPa @Strain 3.3 %, Temperature -40.0 °C | 12040 psi @Strain 3.3 %, Temperature -40.0 °F |
| 84.08 MPa @Strain 3.4 %, Temperature -40.0 °C | 12190 psi @Strain 3.4 %, Temperature -40.0 °F |
| 85.3 MPa @Strain 3.5 %, Temperature -40.0 °C | 12400 psi @Strain 3.5 %, Temperature -40.0 °F |
| 86.4 MPa @Strain 3.6 %, Temperature -40.0 °C | 12500 psi @Strain 3.6 %, Temperature -40.0 °F |
| 87.44 MPa @Strain 3.7 %, Temperature -40.0 °C | 12680 psi @Strain 3.7 %, Temperature -40.0 °F |
| 88.37 MPa @Strain 3.8 %, Temperature -40.0 °C | 12820 psi @Strain 3.8 %, Temperature -40.0 °F |
| 89.07 MPa @Strain 3.9 %, Temperature -40.0 °C | 12920 psi @Strain 3.9 %, Temperature -40.0 °F |
| 89.53 MPa @Strain 4 %, Temperature -40.0 °C | 12990 psi @Strain 4 %, Temperature -40.0 °F |
| 90.4 MPa @Strain 4.1 %, Temperature -40.0 °C | 13100 psi @Strain 4.1 %, Temperature -40.0 °F |
| 90.69 MPa @Strain 4.2 %, Temperature -40.0 °C | 13150 psi @Strain 4.2 %, Temperature -40.0 °F |
| 91.22 MPa @Strain 4.3 %, Temperature -40.0 °C | 13230 psi @Strain 4.3 %, Temperature -40.0 °F |
| 91.74 MPa @Strain 4.4 %, Temperature -40.0 °C | 13310 psi @Strain 4.4 %, Temperature -40.0 °F |
| 92.2 MPa @Strain 4.5 %, Temperature -40.0 °C | 13400 psi @Strain 4.5 %, Temperature -40.0 °F |
| 92.55 MPa @Strain 4.6 %, Temperature -40.0 °C | 13420 psi @Strain 4.6 %, Temperature -40.0 °F |
| 92.84 MPa @Strain 4.7 %, Temperature -40.0 °C | 13470 psi @Strain 4.7 %, Temperature -40.0 °F |
| 93.25 MPa @Strain 4.8 %, Temperature -40.0 °C | 13520 psi @Strain 4.8 %, Temperature -40.0 °F |
| 93.54 MPa @Strain 4.9 %, Temperature -40.0 °C | 13570 psi @Strain 4.9 %, Temperature -40.0 °F |
| 93.71 MPa @Strain 5.0 %, Temperature -40.0 °C | 13590 psi @Strain 5.0 %, Temperature -40.0 °F |
| 94.57 MPa @Strain 35 %, Temperature -40.0 °C | 13720 psi @Strain 35 %, Temperature -40.0 °F |
| 94.85 MPa @Strain 33 %, Temperature -40.0 °C | 13760 psi @Strain 33 %, Temperature -40.0 °F |
| 94.89 MPa @Strain 34 %, Temperature -40.0 °C | 13760 psi @Strain 34 %, Temperature -40.0 °F |
| 94.99 MPa @Strain 32 %, Temperature -40.0 °C | 13780 psi @Strain 32 %, Temperature -40.0 °F |
| 95.11 MPa @Strain 5.5 %, Temperature -40.0 °C | 13790 psi @Strain 5.5 %, Temperature -40.0 °F |
| 95.31 MPa @Strain 31 %, Temperature -40.0 °C | 13820 psi @Strain 31 %, Temperature -40.0 °F |
| 95.38 MPa @Strain 30 %, Temperature -40.0 °C | 13830 psi @Strain 30 %, Temperature -40.0 °F |
| 95.67 MPa @Strain 29 %, Temperature -40.0 °C | 13880 psi @Strain 29 %, Temperature -40.0 °F |
| 96.08 MPa @Strain 28 %, Temperature -40.0 °C | 13940 psi @Strain 28 %, Temperature -40.0 °F |
| 96.2 MPa @Strain 27 %, Temperature -40.0 °C | 14000 psi @Strain 27 %, Temperature -40.0 °F |
| 96.5 MPa @Strain 6.0 %, Temperature -40.0 °C | 14000 psi @Strain 6.0 %, Temperature -40.0 °F |
| 96.62 MPa @Strain 26 %, Temperature -40.0 °C | 14010 psi @Strain 26 %, Temperature -40.0 °F |
| 96.88 MPa @Strain 24 %, Temperature -40.0 °C | 14050 psi @Strain 24 %, Temperature -40.0 °F |
| 96.92 MPa @Strain 6.5 %, Temperature -40.0 °C | 14060 psi @Strain 6.5 %, Temperature -40.0 °F |
| 97.07 MPa @Strain 25 %, Temperature -40.0 °C | 14080 psi @Strain 25 %, Temperature -40.0 °F |
| 97.24 MPa @Strain 7.0 %, Temperature -40.0 °C | 14100 psi @Strain 7.0 %, Temperature -40.0 °F |
| 97.35 MPa @Strain 23 %, Temperature -40.0 °C | 14120 psi @Strain 23 %, Temperature -40.0 °F |
| 97.48 MPa @Strain 21 %, Temperature -40.0 °C | 14140 psi @Strain 21 %, Temperature -40.0 °F |
| 97.62 MPa @Strain 9.0 %, Temperature -40.0 °C | 14160 psi @Strain 9.0 %, Temperature -40.0 °F |
| 97.68 MPa @Strain 7.5 %, Temperature -40.0 °C | 14170 psi @Strain 7.5 %, Temperature -40.0 °F |
| 97.72 MPa @Strain 22 %, Temperature -40.0 °C | 14170 psi @Strain 22 %, Temperature -40.0 °F |
| 97.78 MPa @Strain 8.5 %, Temperature -40.0 °C | 14180 psi @Strain 8.5 %, Temperature -40.0 °F |
| 97.83 MPa @Strain 8.0 %, Temperature -40.0 °C | 14190 psi @Strain 8.0 %, Temperature -40.0 °F |
| 97.86 MPa @Strain 16 %, Temperature -40.0 °C | 14190 psi @Strain 16 %, Temperature -40.0 °F |
| 97.93 MPa @Strain 20 %, Temperature -40.0 °C | 14200 psi @Strain 20 %, Temperature -40.0 °F |
| 98.13 MPa @Strain 15 %, Temperature -40.0 °C | 14230 psi @Strain 15 %, Temperature -40.0 °F |
| 98.14 MPa @Strain 11 %, Temperature -40.0 °C | 14230 psi @Strain 11 %, Temperature -40.0 °F |
| 98.17 MPa @Strain 9.5 %, Temperature -40.0 °C | 14240 psi @Strain 9.5 %, Temperature -40.0 °F |
| 98.46 MPa @Strain 10 %, Temperature -40.0 °C | 14280 psi @Strain 10 %, Temperature -40.0 °F |
| 98.5 MPa @Strain 14 %, Temperature -40.0 °C | 14300 psi @Strain 14 %, Temperature -40.0 °F |
| 98.59 MPa @Strain 19 %, Temperature -40.0 °C | 14300 psi @Strain 19 %, Temperature -40.0 °F |
| 98.86 MPa @Strain 12 %, Temperature -40.0 °C | 14340 psi @Strain 12 %, Temperature -40.0 °F |
| 98.99 MPa @Strain 13 %, Temperature -40.0 °C | 14360 psi @Strain 13 %, Temperature -40.0 °F |
| 99.38 MPa @Strain 18 %, Temperature -40.0 °C | 14410 psi @Strain 18 %, Temperature -40.0 °F |
| 99.53 MPa @Strain 17 %, Temperature -40.0 °C | 14440 psi @Strain 17 %, Temperature -40.0 °F |
Elongation at Break | 20 % @Temperature 23.0 °C | 20 % @Temperature 73.4 °F |
| 27 % @Temperature 23.0 °C | 27 % @Temperature 73.4 °F |
Elongation at Yield | 12 % @Temperature 23.0 °C | 12 % @Temperature 73.4 °F |
Tensile Modulus | 3.40 GPa @Temperature 23.0 °C | 493 ksi @Temperature 73.4 °F |
Flexural Modulus | 3.10 GPa @Temperature 23.0 °C | 450 ksi @Temperature 73.4 °F |
Izod Impact, Notched (ISO) | 7.00 kJ/m² @Temperature 23.0 °C | 3.33 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | 17.0 J/cm² @Temperature -30.0 °C | 80.9 ft-lb/in² @Temperature -22.0 °F |
| 17.0 J/cm² @Temperature 23.0 °C | 80.9 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 0.600 J/cm² @Temperature -30.0 °C | 2.86 ft-lb/in² @Temperature -22.0 °F |
| 0.700 J/cm² @Temperature 23.0 °C | 3.33 ft-lb/in² @Temperature 73.4 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 500 µm/m-°C @Temperature -40.0 - 23.0 °C | 278 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 500 µm/m-°C @Temperature 23.0 - 55.0 °C | 278 µin/in-°F @Temperature 73.4 - 131 °F |
| 500 µm/m-°C @Temperature 55.0 - 100 °C | 278 µin/in-°F @Temperature 131 - 212 °F |
CTE, linear, Transverse to Flow | 90.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 50.0 µin/in-°F @Temperature -40.0 - 73.4 °F |
| 100 µm/m-°C @Temperature 23.0 - 55.0 °C | 55.6 µin/in-°F @Temperature 73.4 - 131 °F |
| 140 µm/m-°C @Temperature 55.0 - 100 °C | 77.8 µin/in-°F @Temperature 131 - 212 °F |
Melting Point | 178 °C | 352 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 165 °C | 329 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 105 °C | 221 °F |
UL RTI, Electrical | 50.0 °C @Thickness 0.750 mm | 122 °F @Thickness 0.0295 in |
| 110 °C @Thickness 1.50 mm | 230 °F @Thickness 0.0591 in |
| 110 °C @Thickness 3.00 mm | 230 °F @Thickness 0.118 in |
UL RTI, Mechanical with Impact | 50.0 °C @Thickness 0.750 mm | 122 °F @Thickness 0.0295 in |
| 85.0 °C @Thickness 1.50 mm | 185 °F @Thickness 0.0591 in |
| 90.0 °C @Thickness 3.00 mm | 194 °F @Thickness 0.118 in |
UL RTI, Mechanical without Impact | 50.0 °C @Thickness 0.750 mm | 122 °F @Thickness 0.0295 in |
| 90.0 °C @Thickness 1.50 mm | 194 °F @Thickness 0.0591 in |
| 95.0 °C @Thickness 3.00 mm | 203 °F @Thickness 0.118 in |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
| HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Oxygen Index | 21 % | 21 % |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 215 °C | 419 °F |
| 210 - 220 °C | 410 - 428 °F |
Mold Temperature | 90.0 °C | 194 °F |
| 80.0 - 100 °C | 176 - 212 °F |
Drying Temperature | 80.0 °C | 176 °F |
Dry Time | 2.00 - 4.00 hour | 2.00 - 4.00 hour |
Moisture Content | <= 0.20 % | <= 0.20 % |
|
Descriptive Properties |
---|
Appearance | Black Color |
Drying Recommended | Not normally required unless moisture content of resin exceeds recommended level |
Extrudable - Cast Film | Yes |
Extrudable - Sheet | Yes |
Extrudable - Tubing | Yes |
Extrudable - Wire and Cable | Yes |
Features | Creep Resistance, Good |
| Dimensional Stability, Good |
| Fatigue Resistant |
| Homopolymer |
| Stiffness, High |
| Strength, High |
| Viscosity, Medium |
Forms | Pellets |
Generic | Acetal (POM) Homopolymer |
Material Status | Current |
Part Marking Code | >POM< |
Polymer Family | POM |
Polymer Type | POM Homopolymer |
Processing Method | Injection Molding |
Product Category | Unreinforced Resins |
Region Available - Global | Yes |
Resin Identification | POM |
Ultrasonic Weldable | Yes |
Uses | Automotive Applications |
| Fasteners |
| Gears |
| Irrigation Applications |
| Parts, Engineering |