Envalior Novamid® 1013GMF H2 NAT/BK37 PA6-GF30
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 30% Glass Fiber Filled
Material Notes:
30% Glass Reinforced, Heat Stabilized, Injection Molding, Excellent Dimensional Stability
Former DSM Engineering Plastics product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.36
g/cc
0.0491
lb/in³
dry; ISO 1183
Moisture Absorption
2.40 %
2.40 %
Sim. To ISO 62
Linear Mold Shrinkage, Flow
0.0070
cm/cm
0.0070
in/in
Sim. To ISO 294-4
Linear Mold Shrinkage, Transverse
0.0080
cm/cm
0.0080
in/in
Sim. To ISO 294-4
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
67.0
MPa
9720
psi
cond; ISO 527-1/-2
135
MPa
19600
psi
dry; ISO 527-1/-2
Elongation at Break
3.6 %
3.6 %
dry; ISO 527-1/-2
8.2 %
8.2 %
cond; ISO 527-1/-2
Tensile Modulus
3.70
GPa
537
ksi
cond; ISO 527-1/-2
7.20
GPa
1040
ksi
dry; ISO 527-1/-2
Flexural Strength
110
MPa
16000
psi
cond; ISO 178
210
MPa
30500
psi
dry; ISO 178
Flexural Modulus
3.10
GPa
450
ksi
cond; ISO 178
6.60
GPa
957
ksi
dry; ISO 178
Charpy Impact Unnotched
5.80
J/cm²
@Temperature 23.0 °C
27.6
ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eU
7.80
J/cm²
@Temperature 23.0 °C
37.1
ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eU
Charpy Impact, Notched
0.600
J/cm²
@Temperature 23.0 °C
2.86
ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eA
1.30
J/cm²
@Temperature 23.0 °C
6.19
ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eA
Thermal Properties
Metric
English
Comments
Melting Point
220
°C
428
°F
10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi)
210
°C
410
°F
dry; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi)
165
°C
329
°F
dry; ISO 75-1/-2
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
DuPont Mobility and Materials Zytel® 73G30HSL BK261 PA6-GF30
Celanese Celstran® PA6-GF30-01 Nylon 6, 30% Glass Reinforced
Envalior Novamid® 1013GH30 1 NA/BK701 PA6-GF30
Envalior Novamid® 1013G30 1 NA PA6-GF30
Celanese Zytel® 73G30HSL NC010 PA6-GF30
PDSM9865 / 161486
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.