MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celanex® 3300LM PBT, 30% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Material Notes: Celanex 3300LM is a 30% glass reinforced lasermarkable grade specially formulated to yield crisp marks when subjected to a Nd:YAG laser or equivalent operated at 1064nm or 532nm. Lasers operating in the UV region (355nm) may yield different results3300LM also offers a superior combination of mechanical, electrical, and thermal properties. This grade provides outstanding processability and good chemical resistance.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.53 g/cc1.53 g/ccASTM D792
Density 1.53 g/cc0.0553 lb/in³ISO 1183
Moisture Absorption 0.200 %0.200 %23°C/50%RH; ISO 62
Linear Mold Shrinkage, Flow 0.0020 - 0.0050 cm/cm0.0020 - 0.0050 in/inISO 294-4
 0.0030 - 0.0050 cm/cm0.0030 - 0.0050 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.014 - 0.021 cm/cm0.014 - 0.021 in/inISO 294-4
Melt Flow 17 g/10 min
@Load 2.16 kg,
Temperature 250 °C
17 g/10 min
@Load 4.76 lb,
Temperature 482 °F
[cm3/10min]; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9090ISO 2039-2
Tensile Strength at Break 130 MPa18900 psi5mm/min; ISO 527-2/1A
 134 MPa19500 psiASTM D638
Elongation at Break 2.0 %2.0 %ASTM D638
 2.5 %2.5 %5mm/min; ISO 527-2/1A
Tensile Modulus 9.20 GPa1330 ksi50mm/min; ISO 527-2/1A
Flexural Strength 193 MPa28000 psiASTM D790
 210 MPa30500 psiISO 178
Flexural Modulus 8.27 GPa1200 ksiASTM D790
 9.70 GPa1410 ksiISO 178
Izod Impact, Notched 0.908 J/cm1.70 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 7.50 kJ/m²3.57 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched 4.60 J/cm²21.9 ft-lb/in²ISO 179/1eU
 4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.850 J/cm²4.04 ft-lb/in²ISO 179/1eA
 0.850 J/cm²
@Temperature -30.0 °C
4.04 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  4.1
@Frequency 1e+6 Hz
4.1
@Frequency 1e+6 Hz
IEC 60250
 4.5
@Frequency 100 Hz
4.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 31.0 kV/mm787 kV/inIEC 60243-1
Dissipation Factor  0.0022
@Frequency 100 Hz
0.0022
@Frequency 100 Hz
IEC 60250
 0.016
@Frequency 1e+6 Hz
0.016
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 425 V425 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 25.0 µm/m-°C13.9 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°C55.6 µin/in-°FISO 11359-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1,-2,-3
 225 °C437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 225 °C437 °FISO 75-1, -2
 228 °C442 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FISO 75-1, -2
 206 °C403 °FASTM D648
Vicat Softening Point 220 °C428 °FISO 306
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-1,-2,-3
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Processing Temperature 65.0 - 93.0 °C149 - 199 °Fcavity
 250 - 260 °C482 - 500 °Fhot runner
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 250 - 260 °C482 - 500 °F
Melt Temperature 235 - 260 °C455 - 500 °F
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4.00 hour4.00 hour
Moisture Content <= 0.020 %<= 0.020 %
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Celanex® 2300 GV1/20 PBT, 20% Glass Reinforced
INEOS Styrolution Luran® S KR 2863 C UV Colored ASA+PC
Evonik Vestodur® X4877 30% Glass Reinforced Laser Markable PBT
DuPont Mobility and Materials Crastin® SK615SF BK591 PBT-GF30
Celanese Hostaform® LW15EWX POM, Tribological

PHCQ053 / 178508

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.