MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

AdvanSource Biomaterials ChronoFlex® C 75D Biodurable Medical Grade Polyurethane
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Polycarbonate-Urethane

Material Notes: ChronoFlex® C is a family of premium polycarbonate aromatic biodurable thermoplastic polyurethane elastomers developed by AdvanSource Biomaterials Corporation. ChronoFlex® C medical-grade elastomers are manufactured under strict GMP conditions. Polycarbonate polyurethanes have been shown to minimize surface degradation such as stress induced microfissures. Aromatic materials have good solvent resistance and limited softening in the body.

Information provided by AdvanSource Biomaterials Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ASTM D792
Water Absorption 0.80 %0.80 %ASTM D570
Melt Flow 3.0 g/10 min
@Load 2.17 kg,
Temperature 210 °C
3.0 g/10 min
@Load 4.78 lb,
Temperature 410 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7575
Tensile Strength, Ultimate 48.3 - 55.2 MPa7000 - 8000 psiConditioned 7 days at RT/50% RH; ASTM D638
Elongation at Break 255 - 320 %255 - 320 %Conditioned 7 days at RT/50% RH; ASTM D638
100% Modulus 36.5 - 39.3 MPa
@Strain 100 %
5300 - 5700 psi
@Strain 100 %
Secant; Conditioned 7 days at RT/50% RH; ASTM D638
300% Modulus 18.6 - 22.1 MPa
@Strain 300 %
2700 - 3200 psi
@Strain 300 %
Secant; Conditioned 7 days at RT/50% RH; ASTM D638
Flexural Strength 6.89 MPa1000 psiASTM D790
Flexural Modulus 0.207 GPa30.0 ksiASTM D790
Coefficient of Friction, Dynamic 0.640.64ASTM D1894
Abrasion 0.0530.053% loss/1000 cycles; ASTM D1044
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 16.5 kV/mm420 kV/inASTM D149
 
Processing PropertiesMetricEnglishComments
Zone 1 216 °C420 °F
Zone 2 224 °C435 °F
Zone 3 232 °C450 °F
Die Temperature 238 °C460 °F
Melt Temperature 238 °C460 °F
Drying Temperature 96.1 - 116 °C205 - 240 °F
Dry Time 3 - 4 hour3 - 4 hour
Moisture Content <= 0.10 %<= 0.10 %
Dew Point -40.0 °C-40.0 °F
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYesU.S.P. XXII
 
Descriptive Properties
AppearanceClear to slightly cloudy
Recommended SterilizationGamma, E-Beam, Ethylene Oxide

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AdvanSource Biomaterials ChronoFlex® C 80A Biodurable Medical Grade Polyurethane
ATI Allvac® Vasco® 316-L Specialty Steel, Heat Treatment: 1038°C (1900°F) Anneal
AdvanSource Biomaterials ChronoFlex® C 55D Biodurable Medical Grade Polyurethane
AdvanSource Biomaterials ChronoPrene™ 25A Thermoplastic Rubber Elastomer
AdvanSource Biomaterials ChronoFlex® AL 65D Biodurable Medical Grade Polyurethane

PCARDI06 / 27930

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.