MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 6, Glass/Mineral Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Glass/Mineral Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Glass/Mineral Reinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.14 - 2.00 g/cc0.0412 - 0.0723 lb/in³Average value: 1.44 g/cc Grade Count:325
 1.289 - 1.289 g/cc
@Temperature >=220 °C
0.04657 - 0.04657 lb/in³
@Temperature >=428 °F
Average value: 1.29 g/cc Grade Count:1
Filler Content 10.0 - 45.0 %10.0 - 45.0 %Average value: 32.7 % Grade Count:44
Water Absorption 0.0900 - 8.00 %0.0900 - 8.00 %Average value: 2.87 % Grade Count:110
Moisture Absorption at Equilibrium 0.800 - 5.70 %0.800 - 5.70 %Average value: 1.96 % Grade Count:100
 1.40 - 1.40 %
@Temperature 70.0 - 70.0 °C
1.40 - 1.40 %
@Temperature 158 - 158 °F
Average value: 1.40 % Grade Count:2
Water Absorption at Saturation 3.50 - 8.00 %3.50 - 8.00 %Average value: 5.81 % Grade Count:36
Viscosity  100000 - 125000 cP
@Temperature 100 - 1000 °C
100000 - 125000 cP
@Temperature 212 - 1830 °F
Average value: 117000 cP Grade Count:3
 100000 - 125000 cP
@Pressure 1.79 - 1.93 MPa
100000 - 125000 cP
@Pressure 260 - 280 psi
Average value: 117000 cP Grade Count:3
Viscosity Number 130 - 160 cm³/g1.30 - 1.60 dl/gAverage value: 143 cm³/g Grade Count:6
Maximum Moisture Content 0.150 - 0.2000.150 - 0.200Average value: 0.178 Grade Count:9
Linear Mold Shrinkage 0.00100 - 0.0150 cm/cm0.00100 - 0.0150 in/inAverage value: 0.00474 cm/cm Grade Count:241
 0.00400 - 0.00400 cm/cm
@Temperature 80.0 - 80.0 °C
0.00400 - 0.00400 in/in
@Temperature 176 - 176 °F
Average value: 0.00400 cm/cm Grade Count:1
Linear Mold Shrinkage, Transverse 0.00110 - 0.0189 cm/cm0.00110 - 0.0189 in/inAverage value: 0.00773 cm/cm Grade Count:133
 0.00800 - 0.00800 cm/cm
@Temperature 80.0 - 80.0 °C
0.00800 - 0.00800 in/in
@Temperature 176 - 176 °F
Average value: 0.00800 cm/cm Grade Count:1
Melt Flow 2.00 - 150 g/10 min2.00 - 150 g/10 minAverage value: 33.5 g/10 min Grade Count:39
Ash 15.0 - 42.0 %15.0 - 42.0 %Average value: 33.4 % Grade Count:14
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 78.0 - 12178.0 - 121Average value: 100 Grade Count:5
Hardness, Rockwell R 115 - 122115 - 122Average value: 120 Grade Count:41
Ball Indentation Hardness 80.0 - 320 MPa11600 - 46400 psiAverage value: 179 MPa Grade Count:21
Tensile Strength, Ultimate 45.0 - 200 MPa6530 - 29000 psiAverage value: 103 MPa Grade Count:274
 25.0 - 178 MPa
@Temperature -40.0 - 150 °C
3630 - 25800 psi
@Temperature -40.0 - 302 °F
Average value: 70.3 MPa Grade Count:9
Tensile Strength, Yield 40.0 - 186 MPa5800 - 27000 psiAverage value: 105 MPa Grade Count:50
Elongation at Break 1.00 - 183 %1.00 - 183 %Average value: 4.50 % Grade Count:286
 1.80 - 25.0 %
@Temperature -40.0 - 150 °C
1.80 - 25.0 %
@Temperature -40.0 - 302 °F
Average value: 6.51 % Grade Count:7
Elongation at Yield 1.80 - 22.6 %1.80 - 22.6 %Average value: 4.71 % Grade Count:17
Modulus of Elasticity 0.600 - 20.8 GPa87.0 - 3020 ksiAverage value: 6.97 GPa Grade Count:169
 1.70 - 10.79 GPa
@Temperature -40.0 - 150 °C
247 - 1565 ksi
@Temperature -40.0 - 302 °F
Average value: 4.32 GPa Grade Count:8
Flexural Yield Strength 50.0 - 290 MPa7250 - 42100 psiAverage value: 163 MPa Grade Count:223
 70.0 - 245 MPa
@Temperature -40.0 - 90.0 °C
10200 - 35500 psi
@Temperature -40.0 - 194 °F
Average value: 137 MPa Grade Count:2
Flexural Modulus 0.640 - 14.1 GPa92.8 - 2050 ksiAverage value: 6.94 GPa Grade Count:251
 2.40 - 8.40 GPa
@Temperature -40.0 - 120 °C
348 - 1220 ksi
@Temperature -40.0 - 248 °F
Average value: 4.30 GPa Grade Count:3
Flexural Strain at Break 1.50 - 8.00 %1.50 - 8.00 %Average value: 4.25 % Grade Count:22
Compressive Yield Strength 89.6 - 159 MPa13000 - 23100 psiAverage value: 119 MPa Grade Count:8
Izod Impact, Notched 0.300 - 2.14 J/cm0.562 - 4.00 ft-lb/inAverage value: 0.704 J/cm Grade Count:97
 0.280 - 0.700 J/cm
@Temperature -40.0 - -20.0 °C
0.525 - 1.31 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 0.336 J/cm Grade Count:5
 0.186865 - 0.186865 J/cm
@Temperature -40.0 - -40.0 °C
0.350075 - 0.350075 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 0.336 J/cm Grade Count:2
 0.186865 - 0.186865 J/cm
@Thickness 3.17 - 3.17 mm
0.350075 - 0.350075 ft-lb/in
@Thickness 0.125 - 0.125 in
Average value: 0.336 J/cm Grade Count:2
Izod Impact, Unnotched 3.74 J/cm - NB7.00 ft-lb/in - NBAverage value: 5.83 J/cm Grade Count:18
Izod Impact, Notched (ISO) 2.40 - 16.0 kJ/m²1.14 - 7.61 ft-lb/in²Average value: 6.57 kJ/m² Grade Count:113
 3.00 - 10.0 kJ/m²
@Temperature -40.0 - -30.0 °C
1.43 - 4.76 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 7.58 kJ/m² Grade Count:31
Izod Impact, Unnotched (ISO) 22.0 kJ/m² - NB10.5 ft-lb/in² - NBAverage value: 45.0 kJ/m² Grade Count:24
 25.0 - 50.0 kJ/m²
@Temperature -30.0 - -30.0 °C
11.9 - 23.8 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 33.8 kJ/m² Grade Count:14
Charpy Impact Unnotched 1.50 J/cm² - NB7.14 ft-lb/in² - NBAverage value: 4.58 J/cm² Grade Count:137
 1.30 J/cm² - NB
@Temperature -40.0 - -20.0 °C
6.19 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 3.61 J/cm² Grade Count:86
Charpy Impact, Notched 0.200 - 6.00 J/cm²0.952 - 28.6 ft-lb/in²Average value: 0.662 J/cm² Grade Count:177
 0.150 - 1.10 J/cm²
@Temperature -40.0 - -20.0 °C
0.714 - 5.24 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 0.510 J/cm² Grade Count:83
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+9 - 1.00e+16 ohm-cm1.00e+9 - 1.00e+16 ohm-cmAverage value: 3.81e+14 ohm-cm Grade Count:104
Surface Resistance 440 - 1.00e+16 ohm440 - 1.00e+16 ohmAverage value: 3.47e+14 ohm Grade Count:58
Dielectric Constant 3.00 - 14.03.00 - 14.0Average value: 5.47 Grade Count:67
Dielectric Strength 7.87 - 90.0 kV/mm200 - 2290 kV/inAverage value: 27.5 kV/mm Grade Count:80
Dissipation Factor 0.00100 - 0.4000.00100 - 0.400Average value: 0.0873 Grade Count:52
Dielectric Loss Index 0.0200 - 0.2000.0200 - 0.200Average value: 0.110 Grade Count:6
Arc Resistance 100 - 130 sec100 - 130 secAverage value: 120 sec Grade Count:7
Comparative Tracking Index 225 - 600 V225 - 600 VAverage value: 485 V Grade Count:57
 
Thermal PropertiesMetricEnglishComments
CTE, linear 14.4 - 110 µm/m-°C8.00 - 61.1 µin/in-°FAverage value: 35.9 µm/m-°C Grade Count:66
CTE, linear, Transverse to Flow 34.0 - 104 µm/m-°C18.9 - 57.8 µin/in-°FAverage value: 68.3 µm/m-°C Grade Count:34
Specific Heat Capacity 1.30 - 2.03 J/g-°C0.311 - 0.485 BTU/lb-°FAverage value: 1.43 J/g-°C Grade Count:7
Thermal Conductivity 0.250 - 1.10 W/m-K1.74 - 7.63 BTU-in/hr-ft²-°FAverage value: 0.618 W/m-K Grade Count:11
Melting Point 200 - 315 °C392 - 599 °FAverage value: 222 °C Grade Count:211
Maximum Service Temperature, Air 80.0 - 200 °C176 - 392 °FAverage value: 149 °C Grade Count:23
Deflection Temperature at 0.46 MPa (66 psi) 75.0 - 307 °C167 - 585 °FAverage value: 212 °C Grade Count:122
Deflection Temperature at 1.8 MPa (264 psi) 55.0 - 290 °C131 - 554 °FAverage value: 192 °C Grade Count:244
Deflection Temperature at 8.0 MPa 50.0 - 140 °C122 - 284 °FAverage value: 77.5 °C Grade Count:10
Vicat Softening Point 165 - 230 °C329 - 446 °FAverage value: 205 °C Grade Count:48
Minimum Service Temperature, Air -100 - -40.0 °C-148 - -40.0 °FAverage value: -65.0 °C Grade Count:3
UL RTI, Electrical 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
UL RTI, Mechanical with Impact 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
UL RTI, Mechanical without Impact 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
Flammability, UL94 HB - V-0HB - V-0Grade Count:108
 V-0 - V-0
@Temperature 1.50 - 1.50 °C
V-0 - V-0
@Temperature 34.7 - 34.7 °F
Grade Count:1
Flame Spread 0.000 mm/min0.000 in/minAverage value: 0.000 mm/min Grade Count:3
Oxygen Index 22.0 - 68.0 %22.0 - 68.0 %Average value: 36.4 % Grade Count:16
Glow Wire Test 650 - 960 °C1200 - 1760 °FAverage value: 816 °C Grade Count:25
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 300 °C176 - 572 °FAverage value: 252 °C Grade Count:18
Nozzle Temperature 210 - 293 °C410 - 560 °FAverage value: 265 °C Grade Count:25
Melt Temperature 216 - 330 °C420 - 626 °FAverage value: 268 °C Grade Count:145
Mold Temperature 26.7 - 140 °C80.0 - 284 °FAverage value: 82.9 °C Grade Count:152
Drying Temperature 60.0 - 120 °C140 - 248 °FAverage value: 83.6 °C Grade Count:86
Moisture Content 0.0300 - 0.200 %0.0300 - 0.200 %Average value: 0.144 % Grade Count:42
Injection Pressure 4.96 - 150 MPa720 - 21800 psiAverage value: 80.8 MPa Grade Count:37

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Mineral Reinforced, Impact Grade
Overview of materials for Nylon 6, 30% Mineral Filled
Overview of materials for Nylon 66/6, Mineral Reinforced
Overview of materials for Nylon 6, 20% Mineral Filled
Overview of materials for Nylon 6, 40% Mineral Filled

O2429 / 77986

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.