MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Phosphor bronze 5% Sn, UNS C51000, OSO50 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Excellent cold workability. Fabricated by blanking, drawing, bending, heading, and upsetting, shearing, roll threading, knurling and stamping.

Applications: bellows, bourdon tubing, clutch discs, cotter pins, diaphragms, fasteners, lock washers, wire brushes, chemical hardware, textile machinery, welding rod.

Trace content of Phosphorus.

Test specimen: flat products - 1mm thickness.

Key Words: CDA 510, PB102, ISO CuSn5
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.86 g/cc0.320 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 2626
Tensile Strength, Ultimate 325 MPa47100 psi
Tensile Strength, Yield 130 MPa
@Strain 0.5 %
18900 psi
@Strain 0.5 %
Elongation at Break 64 %64 %In 50 mm
Modulus of Elasticity 110 GPa16000 ksi
Poissons Ratio 0.3410.341
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 41.0 GPa5950 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000870 ohm-cm
@Temperature 20.0 °C
0.00000870 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 17.8 µm/m-°C
@Temperature 20.0 - 300 °C
9.89 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.380 J/g-°C0.0908 BTU/lb-°F
Thermal Conductivity 84.0 W/m-K
@Temperature 20.0 °C
583 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 975 - 1060 °C1790 - 1940 °F
Solidus 975 °C1790 °F
Liquidus 1060 °C1940 °F
Annealing Point 482 - 677 °C900 - 1250 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 475 - 675 °C887 - 1250 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 93.6 - 95.6 %93.6 - 95.6 %
Iron, Fe <= 0.10 %<= 0.10 %
Lead, Pb <= 0.050 %<= 0.050 %
Phosphorus, P 0.030 - 0.35 %0.030 - 0.35 %
Tin, Sn 4.2 - 5.8 %4.2 - 5.8 %
Zinc, Zn <= 0.30 %<= 0.30 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Phosphor bronze 5% Sn, UNS C51000
Phosphor bronze 5% Sn, UNS C51000, OSO35 Temper flat products
Phosphor bronze 5% Sn, UNS C51000, OSO25 Temper flat products
Phosphor bronze 5% Sn, UNS C51000, H02 Temper flat products
Phosphor bronze 5% Sn, UNS C51000, OSO15 Temper flat products

MC51000b2 / 11504

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.