MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

Magnesium, Mg; Annealed Sheet
Categories: Metal; Nonferrous Metal; Magnesium Alloy; Pure Element

Material Notes: Annealed applies only to tensile and/or hardness values; other property values are typical of the element. This entry is for pure Mg; MatWeb has over 125 Mg alloys entries too.

Magnesium alloys are very low density (1.7 g/cc) and can be treated to reasonably high strengths. Magnesium alloys are available in both wrought and cast forms. Its low density

Many Mg alloys are listed in MatWeb.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.74 g/cc0.0629 lb/in³
Viscosity  1.13 cP
@Temperature 700 °C
1.13 cP
@Temperature 1290 °F
 1.23 cP
@Temperature 650 °C
1.23 cP
@Temperature 1200 °F
a Lattice Constant 3.209 Å3.209 Å
c Lattice Constant 5.211 Å5.211 Å
Vapor Pressure  1.51987e-020 bar
@Temperature 25.000 °C
1.00e-17 torr
@Temperature 77.000 °F
 5.27e-14 bar
@Temperature 127 °C
3.95e-11 torr
@Temperature 260 °F
 0.00360 bar
@Temperature 650 °C
2.70 torr
@Temperature 1200 °F
solid and liquid
 
Chemical PropertiesMetricEnglishComments
Atomic Mass 24.305024.30501995
Atomic Number 1212
Thermal Neutron Cross Section 0.060 barns/atom0.060 barns/atom
X-ray Absorption Edge 9.5117 Å9.5117 ÅK
 197.39 Å197.39 ÅLI
 247.92 Å247.92 ÅLII
 247.92 Å247.92 ÅLIII
Electrode Potential -2.37 V-2.37 V
Electronegativity 1.311.31Pauling
Ionic Radius 0.660 Å0.660 ÅCrystal Ionic Radius for Valence +2
 0.820 Å0.820 ÅCrystal Ionic Radius for Valence +1
Electrochemical Equivalent 0.454 g/A/h0.454 g/A/h
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 4040500 kg load/10 mm ball
Tensile Strength, Ultimate 160 - 196 MPa23200 - 28400 psi
Tensile Strength, Yield 90.0 - 105 MPa13100 - 15200 psi
Elongation at Break 3.0 - 15 %3.0 - 15 %
Modulus of Elasticity 44.0 GPa6380 ksi
Compressive Yield Strength 69.0 - 83.0 MPa10000 - 12000 psi
Poissons Ratio 0.350.35
Shear Modulus 16.3 GPa2360 ksiCalculated
Coefficient of Friction 0.360.36versus magnesium at 20°C
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000460 ohm-cm0.00000460 ohm-cm
Magnetic Permeability 1.000011.00001
Magnetic Susceptibility 5.5e-75.5e-7cgs/g
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 371.8 J/g159.9 BTU/lb
Heat of Vaporization 4760 J/g2050 BTU/lb
CTE, linear  26.1 µm/m-°C
@Temperature 20.0 - 100 °C
14.5 µin/in-°F
@Temperature 68.0 - 212 °F
 27.2 µm/m-°C
@Temperature 250 °C
15.1 µin/in-°F
@Temperature 482 °F
 29.6 µm/m-°C
@Temperature 500 °C
16.4 µin/in-°F
@Temperature 932 °F
Specific Heat Capacity 1.025 J/g-°C0.2450 BTU/lb-°F
Thermal Conductivity 159 W/m-K1100 BTU-in/hr-ft²-°F
Melting Point 648.3 - 649.3 °C1199 - 1201 °F
Boiling Point 1090 °C1990 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.070
@Temperature 22.0 °C
0.070
@Temperature 71.6 °F
Reflection Coefficient, Visible (0-1) 0.740.74at 1.00 micron
 0.72 - 0.770.72 - 0.77at 500 nm
 0.800.80at 3.0 micron
 0.930.93at 9.0 micron
 
Component Elements PropertiesMetricEnglishComments
Magnesium, Mg 100 %100 %
 
Descriptive Properties
CAS Number7439-95-4
Crystal StructureHCPSpace Group P63/mmc

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Magnesium, Mg; Hard-Rolled Sheet
Magnesium, Mg; Sand Cast
Magnesium, Mg; Extruded
Overview of materials for Magnesium Alloy
Magnesium Elektron Elektron® 21 Magnesium Casting Alloy

AMEMg03 / 59

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.