MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chemours Tefzel® HT-2004  (discontinued **)
Categories: Polymer; Thermoplastic; Fluoropolymer; ETFE/ECTFE

Material Notes: The development of technology by DuPont for reinforcing Tefzel ® ETFE fluoropolymer with glass fibers brings to the plastics industry a new opportunity for design. This product, designated Tefzel ® HT-2004, combines the superior mechanical properties resulting from glass-reinforcement with the impressive thermal, chemical, and electrical properties of Tefzel ®.

Chemours was formed from former DuPont performance chemicals businesses, including DuPont Fluoroproducts, in 2015.

Key Words: Ethylene Tetrafluoroethylene Copolymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.86 g/cc1.86 g/cc
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 83.0 MPa12000 psi
Elongation at Break 9.0 %9.0 %
Flexural Modulus 6.55 GPa950 ksi
Izod Impact, Notched 3.7373 J/cm7.0015 ft-lb/in
 1.835 J/cm
@Temperature -60.0 °C
3.438 ft-lb/in
@Temperature -76.0 °F
 NB
@Temperature 121 °C
NB
@Temperature 250 °F
 NB
@Temperature 204 °C
NB
@Temperature 399 °F
Coefficient of Friction, Dynamic 0.310.3110fpm, 100psi
Coefficient of Friction, Static 0.310.31100 psi
 0.340.34500 psi
 0.380.3850 psi
 0.510.5110 psi
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 16.1 kV/mm410 kV/in125 mil
 
Thermal PropertiesMetricEnglishComments
CTE, linear 22.2 µm/m-°C
@Temperature 20.0 °C
12.3 µin/in-°F
@Temperature 68.0 °F
Flammability, UL94 V-0V-0
 
Descriptive Properties
Chemical/Solvent ResistanceExcellent

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chemours Tefzel® 750 Fluoropolymer Resin
Chemours Tefzel® 280 Resin Modified ETFE
Chemours Tefzel® HT-2127 Fluoropolymer Resin
Chemours Tefzel® 210 Resin Modified ETFE
Chemours Tefzel® 207 Resin Modified ETFE

PDU9293 / 33360

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.