MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik SAF 2205 Precision Wire
Categories: Metal; Ferrous Metal; Duplex; Stainless Steel

Material Notes: Sandvik SAF 2205 rig rod for sailing yachts

Sandvik SAF 2205 is a duplex (austenitic/ferritic) stainless steel suitable for service with high resistance against chloride containing environments, surpassing AISI 316 in seawater. The material has high strength, and is thereby very suitable for high strength components in aggressive environments (e.g. rig rod for sailing yachts). Sandvik SAF 2205 in corrosive oil and gas environments

Sandvik SAF 2205 is a duplex (austenitic/ferritic) stainless steel alloy suitable for service in corrosive oil and gas environments.

Information provided by Sandvik

UNS S31803; EN 1.4462

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate >= 1700 MPa>= 247000 psicorrosive environment
 >= 1300 MPa
@Thickness 12.7 mm
>= 189000 psi
@Thickness 0.500 in
 >= 1450 MPa
@Thickness 4.00 mm
>= 210000 psi
@Thickness 0.157 in
Tensile Strength, Yield >= 1530 MPa>= 222000 psicorrosive environment
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000850 ohm-cm0.0000850 ohm-cm
Magnetic Permeability >= 25>= 25
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.0 µm/m-°C
@Temperature 30.0 - 100 °C
7.22 µin/in-°F
@Temperature 86.0 - 212 °F
 13.5 µm/m-°C
@Temperature 30.0 - 200 °C
7.50 µin/in-°F
@Temperature 86.0 - 392 °F
 14.5 µm/m-°C
@Temperature 30.0 - 400 °C
8.06 µin/in-°F
@Temperature 86.0 - 752 °F
Specific Heat Capacity 0.590 J/g-°C0.141 BTU/lb-°F
 0.480 J/g-°C
@Temperature 20.0 °C
0.115 BTU/lb-°F
@Temperature 68.0 °F
 0.530 J/g-°C
@Temperature 200 °C
0.127 BTU/lb-°F
@Temperature 392 °F
Thermal Conductivity  14.0 W/m-K
@Temperature 20.0 °C
97.2 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 17.0 W/m-K
@Temperature 200 °C
118 BTU-in/hr-ft²-°F
@Temperature 392 °F
 20.0 W/m-K
@Temperature 400 °C
139 BTU-in/hr-ft²-°F
@Temperature 752 °F
Maximum Service Temperature, Air 280 °C536 °F
Minimum Service Temperature, Air -50.0 °C-58.0 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 22 %22 %
Iron, Fe 66 %66 %As Balance
Manganese, Mn 2.0 %2.0 %
Molybdenum, Mo 3.2 %3.2 %
Nickel, Ni 5.5 %5.5 %
Nitrogen, N 0.18 %0.18 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.015 %<= 0.015 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sandvik SANMAC SAF 2205 Bar Steel
Sandvik SAF 2205 Billet
Carlson 2205 (UNS S32205) Duplex Stainless Steel
Carlson 2205 (UNS S31803) Duplex Stainless Steel
MetalTek MTEK 2205 Cast UNS J92205 Duplex Stainless Steel

NSANDV216 / 19110

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.