MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Arnite® TV4 230 SF PBT-15% Glass Reinforced (European and Asian Grade)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.

Arnite Molding resins:

  • Standard Unfilled and Reinforced materials
  • High modulus Flame retardant grades
  • Easy molding FR grades for connectors
  • Toughened unfilled materials for durability
  • High modulus, tight specification for critical auto components
  • Toughened reinforced resins
  • Low outgassing grades for reflector surfaces

Arnite extrusion resins: Specialized materials for specific uses

  • PET for medical applications
  • Loose buffer Optical fiber tubing
  • PET for stock shapes

Applications

  • Automotive:Connectors, sensors and E&E parts, Exterior fittings, Gear housings and motors, Brake valve bodies
  • Electrical & Electronic: Telecoms and IT connectors, Bobbins, Low voltage Power distribution, E-motor components, Lightings and Lamp fittings
  • Consumer Durables: Small Appliances
  • Other: Optical fiber tubing

Information provided by DSM.

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Water Absorption 0.30 %0.30 %Sim. to ISO 62
Moisture Absorption at Equilibrium 0.15 %0.15 %Humidity Absorption; Sim. to ISO 62
Melt Flow 22.56 g/10 min
@Load 2.16 kg,
Temperature 250 °C
22.56 g/10 min
@Load 4.76 lb,
Temperature 482 °F
Calculated from Volume Flow Rate of 16 cm3/10min.; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 95.0 MPa13800 psiISO 527-1/-2
Elongation at Break 2.5 %2.5 %ISO 527-1/-2
Tensile Modulus 7.00 GPa1020 ksiISO 527-1/-2
Charpy Impact Unnotched  4.00 J/cm²
@Temperature -30.0 °C
19.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 4.00 J/cm²
@Temperature 23.0 °C
19.0 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.600 J/cm²
@Temperature 23.0 °C
2.86 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
 3.7
@Frequency 100 Hz
3.7
@Frequency 100 Hz
IEC 60250
Dielectric Strength 28.0 kV/mm711 kV/inIEC 60243-1
Dissipation Factor  0.0025
@Frequency 100 Hz
0.0025
@Frequency 100 Hz
IEC 60250
 0.014
@Frequency 1e+6 Hz
0.014
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 V250 VIEC 60112
 250 - 399 V250 - 399 VPLC 2; UL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C
@Temperature 20.0 °C
22.2 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C
@Temperature 20.0 °C
44.4 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °C419 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 190 °C374 °FISO 75-1/-2
UL RTI, Electrical  130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL746B
 130 °C
@Thickness 0.750 mm
266 °F
@Thickness 0.0295 in
UL746B
UL RTI, Mechanical with Impact  140 °C
@Thickness 0.750 mm
284 °F
@Thickness 0.0295 in
UL746B
 140 °C
@Thickness 1.50 mm
284 °F
@Thickness 0.0591 in
UL746B
UL RTI, Mechanical without Impact  130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL746B
 130 °C
@Thickness 0.750 mm
266 °F
@Thickness 0.0295 in
UL746B
Flammability, UL94  V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
IEC 60695-11-10
 V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
IEC 60695-11-10
 5VB
@Thickness 1.50 mm
5VB
@Thickness 0.0591 in
IEC 60695-11-20
Glow Wire Ignition Temperature  725 °C
@Thickness 1.50 mm
1340 °F
@Thickness 0.0591 in
IEC 60695-2-13
 800 °C
@Thickness 0.750 mm
1470 °F
@Thickness 0.0295 in
IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 0.750 mm
1760 °F
@Thickness 0.0295 in
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC 60695-2-12
 
Descriptive Properties
Flame RetardantYes
Flame Retarding AgentYes
Injection MoldingYes
Release AgentYes
With FillersYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Shinkong Synthetic Fibers Shinite® D202G15 PBT, 15% Glass Filled, Fire Retardant
Gromax CCP PBT 4815-NCB 15% Glass Fiber Filled
Shinkong Synthetic Fibers Shinite® E202G15 PBT, 15% Glass Filled
Envalior Arnite® TV4 230 S PBT-GF15 FR(17)
Envalior Arnite® TV4 241 SL PBT-GF20 FR(17)

PDSMEU354 / 31298

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.