MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Covestro Apec® 1745 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: MVR (330°C/2.16kg) 17 cm³/10 min; easy release; suitable for superheated steam sterilisation up to 143 °C as well as for pharmaceutical applications according to United States Pharmacopeia (USP) XXII Class VI; softening temperature (VST/B 120)=170 °C; injection molding - melt temperature 320 - 340°C; Films for medical packaging; Contact lens holders; Medical vessels; Safety valve for respiration aids; Syringe tops

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.17 g/cc0.0423 lb/in³ISO 1183
Melt Density 0.995 g/cc
@Temperature 330 °C
0.0359 lb/in³
@Temperature 626 °F
Moisture Absorption at Equilibrium 0.12 %0.12 %Similar to ISO 62
Water Absorption at Saturation 0.30 %0.30 %Similar to ISO 62
Linear Mold Shrinkage, Flow 0.0080 cm/cm0.0080 in/in60x60x2mm; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/in60x60x2mm; ISO 294-4
Melt Flow 17 g/10 min
@Load 2.16 kg,
Temperature 330 °C
17 g/10 min
@Load 4.76 lb,
Temperature 626 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 120 MPa17400 psiISO 2039-1
Tensile Strength, Yield 70.0 MPa10200 psi50 [mm/min]; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, 50 [mm/min]; ISO 527-1/-2
Elongation at Yield 6.8 %6.8 %50 [mm/min]; ISO 527-1/-2
Tensile Modulus 2.40 GPa348 ksi1 [mm/min]; ISO 527-1/-2
Flexural Strength 105 MPa15200 psi2 [mm/min]; ISO 178
Flexural Modulus 2.40 GPa348 ksi2 [mm/min]; ISO 178
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 60250
 3.0
@Frequency 100 Hz
3.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 35.0 kV/mm889 kV/inIEC 60243-1
Dissipation Factor  0.0010
@Frequency 100 Hz
0.0010
@Frequency 100 Hz
IEC 60250
 0.0080
@Frequency 1e+6 Hz
0.0080
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 125 V125 VM; Solution B; IEC 60112
 250 V250 VSolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
36.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
36.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Deflection Temperature at 0.46 MPa (66 psi) 160 °C320 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 148 °C298 °FISO 75-1/-2
Vicat Softening Point 170 °C
@Load 5.10 kg
338 °F
@Load 11.2 lb
120°C/h; ISO 306
UL RTI, Electrical 140 °C284 °FUL746B
UL RTI, Mechanical with Impact 130 °C266 °FUL746B
UL RTI, Mechanical without Impact 140 °C284 °FUL746B
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
Oxygen Index 25 %25 %Method A; ISO 4589-1/-2
Glow Wire Flammability Index 850 °C1560 °FIEC 60695-2-12
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5781.578Procedure A; ISO 489
Transmission, Visible 88 %88 %1 mm; ISO 13468-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 330 °C626 °FInjection Molding; ISO 294
Mold Temperature 100 °C212 °FInjection Molding; ISO 10724
Injection Velocity 200 mm/sec7.87 in/secISO 294
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes
 
Descriptive Properties
Electrolytic corrosionA1IEC 60426

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chevron Phillips Marlex® 9018 HDPE Injection Molding Resin
Covestro Bayblend® FR 3010 Polycarbonate + ABS, Flame Retardant Grade
Avient Dynaflex™ G7950-1 NSFG Thermoplastic Elastomer (TPE)
Avient Dynaflex™ G7950-1001-00 Thermoplastic Elastomer (TPE)
BASF Elastollan® C 70 A HPM TPUR

PB09702 / 92542

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.