Physical Properties | Metric | English | Comments |
---|
Density | 1.10 g/cc | 0.0397 lb/in³ |
Water Absorption | 1.2 % @Time 86400 sec | 1.2 % @Time 24.0 hour |
Moisture Absorption at Equilibrium | 2.3 % | 2.3 % |
Linear Mold Shrinkage, Flow | 0.018 cm/cm @Thickness 2.00 mm | 0.018 in/in @Thickness 0.0787 in |
Linear Mold Shrinkage, Transverse | 0.016 cm/cm @Thickness 2.00 mm | 0.016 in/in @Thickness 0.0787 in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 38.0 MPa | 5510 psi |
| 57.0 MPa | 8270 psi |
Tensile Strength, Yield | 38.0 MPa | 5510 psi |
| 61.0 MPa | 8850 psi |
Elongation at Break | 22 % | 22 % |
| 108 % | 108 % |
Elongation at Yield | 5.6 % | 5.6 % |
| 41 % | 41 % |
Tensile Modulus | 1.00 GPa | 145 ksi |
| 2.70 GPa | 392 ksi |
Flexural Strength | 24.0 MPa | 3480 psi |
| 70.0 MPa | 10200 psi |
Flexural Modulus | 0.800 GPa | 116 ksi |
| 2.30 GPa | 334 ksi |
Izod Impact, Notched (ISO) | 16.0 kJ/m² @Temperature -30.0 °C | 7.61 ft-lb/in² @Temperature -22.0 °F |
| 18.0 kJ/m² @Temperature 23.0 °C | 8.57 ft-lb/in² @Temperature 73.4 °F |
| 24.0 kJ/m² @Temperature -30.0 °C | 11.4 ft-lb/in² @Temperature -22.0 °F |
| 44.0 kJ/m² @Temperature 23.0 °C | 20.9 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
| NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
Charpy Impact, Notched | 1.10 J/cm² @Temperature -30.0 °C | 5.23 ft-lb/in² @Temperature -22.0 °F |
| 1.60 J/cm² @Temperature 23.0 °C | 7.61 ft-lb/in² @Temperature 73.4 °F |
| 2.40 J/cm² @Temperature -30.0 °C | 11.4 ft-lb/in² @Temperature -22.0 °F |
| 6.20 J/cm² @Temperature 23.0 °C | 29.5 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+11 ohm-cm @Thickness 1.00 mm | 1.00e+11 ohm-cm @Thickness 0.0394 in |
Dielectric Strength | 12.0 kV/mm @Thickness 1.00 mm | 305 kV/in @Thickness 0.0394 in |
Arc Resistance | 60 - 120 sec @Thickness 3.00 mm | 60 - 120 sec @Thickness 0.118 in |
Comparative Tracking Index | 525 V @Thickness 3.00 mm | 525 V @Thickness 0.118 in |
Hot Wire Ignition, HWI | 7.0 - 15 sec | 7.0 - 15 sec |
| 7.0 - 15 sec | 7.0 - 15 sec |
| 15 - 30 sec | 15 - 30 sec |
High Amp Arc Ignition, HAI | >= 120 arcs | >= 120 arcs |
| >= 120 arcs | >= 120 arcs |
| >= 120 arcs | >= 120 arcs |
High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80.0 mm/min | 1.00 - 3.15 in/min |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 110 µm/m-°C @Thickness 2.00 mm, Temperature 35.0 - 55.0 °C | 61.1 µin/in-°F @Thickness 0.0787 in, Temperature 95.0 - 131 °F |
CTE, linear, Transverse to Flow | 140 µm/m-°C @Thickness 2.00 mm, Temperature 23.0 - 55.0 °C | 77.8 µin/in-°F @Thickness 0.0787 in, Temperature 73.4 - 131 °F |
Melting Point | 260 °C | 500 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 185 °C | 365 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 63.0 °C | 145 °F |
UL RTI, Electrical | 130 °C @Thickness 0.750 mm | 266 °F @Thickness 0.0295 in |
| 130 °C @Thickness 1.50 mm | 266 °F @Thickness 0.0591 in |
| 130 °C @Thickness 3.00 mm | 266 °F @Thickness 0.118 in |
UL RTI, Mechanical with Impact | 75.0 °C @Thickness 0.750 mm | 167 °F @Thickness 0.0295 in |
| 75.0 °C @Thickness 1.50 mm | 167 °F @Thickness 0.0591 in |
| 75.0 °C @Thickness 3.00 mm | 167 °F @Thickness 0.118 in |
UL RTI, Mechanical without Impact | 115 °C @Thickness 0.750 mm | 239 °F @Thickness 0.0295 in |
| 115 °C @Thickness 1.50 mm | 239 °F @Thickness 0.0591 in |
| 115 °C @Thickness 3.00 mm | 239 °F @Thickness 0.118 in |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Glow Wire Ignition Temperature | 725 °C @Thickness 0.400 mm | 1340 °F @Thickness 0.0157 in |
| 725 °C @Thickness 1.50 mm | 1340 °F @Thickness 0.0591 in |
| 800 °C @Thickness 0.750 mm | 1470 °F @Thickness 0.0295 in |
Glow Wire Flammability Index | 700 °C @Thickness 0.400 mm | 1290 °F @Thickness 0.0157 in |
| 700 °C @Thickness 1.50 mm | 1290 °F @Thickness 0.0591 in |
| 775 °C @Thickness 0.750 mm | 1430 °F @Thickness 0.0295 in |
|
Processing Properties | Metric | English | Comments |
---|
Rear Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Middle Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Front Barrel Temperature | 280 - 310 °C | 536 - 590 °F |
Nozzle Temperature | 280 - 310 °C | 536 - 590 °F |
Melt Temperature | 285 - 305 °C | 545 - 581 °F |
Mold Temperature | 65.0 - 95.0 °C | 149 - 203 °F |
Drying Temperature | 80.0 °C | 176 °F |
Dry Time | 4.00 hour | 4.00 hour |
|
Descriptive Properties |
---|
Additive | Heat Stabilizer |
Agency Ratings | ASTM, D4066 PA0161 |
| ASTM, D6779 PA0161 |
| SAE, J1639 PA0171 |
Appearance | Black |
Automotive Material Specification | Chery Q-SQR.S1-33-2012 CMP.PA66.A2 |
| Daimler DBL 5410 (compliance) |
| GM GMW16447P-PA66-T2 |
| VW 50180 (compliance) |
Features | Abrasion Resistance |
| Chemical Resistant |
| Gasoline Resistant |
| General Purpose |
| Good Processability |
| Good Toughness |
| Heat Stabilized |
| High Impact Resistance |
| Impact Modified |
| Low Temperature Impact Resistance |
| Low Temperature Toughness |
| Oil Resistant |
| Solvent Resistant |
| Weatherable |
Forms | Pellets |
Outdoor Suitability | f1 |
Processing Method | Injection Molding |
Region | North America, Europe, Asia Pacific |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.