MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Acetal Copolymer, Mineral Filled
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Acetal Copolymer, Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.20 - 1.73 g/cc0.0434 - 0.0625 lb/in³Average value: 1.52 g/cc Grade Count:44
Filler Content 10.0 - 30.0 %10.0 - 30.0 %Average value: 20.0 % Grade Count:4
Water Absorption 0.150 - 0.900 %0.150 - 0.900 %Average value: 0.418 % Grade Count:13
Moisture Absorption at Equilibrium 0.100 - 0.210 %0.100 - 0.210 %Average value: 0.186 % Grade Count:10
Water Absorption at Saturation 0.650 - 0.900 %0.650 - 0.900 %Average value: 0.783 % Grade Count:9
Additive Loading 10.0 - 40.0 %10.0 - 40.0 %Average value: 23.3 % Grade Count:3
Maximum Moisture Content 0.1500.150Average value: 0.150 Grade Count:3
Linear Mold Shrinkage 0.00500 - 0.0270 cm/cm0.00500 - 0.0270 in/inAverage value: 0.0161 cm/cm Grade Count:37
Linear Mold Shrinkage, Transverse 0.0100 - 0.0215 cm/cm0.0100 - 0.0215 in/inAverage value: 0.0154 cm/cm Grade Count:16
Melt Flow 3.80 - 39.0 g/10 min3.80 - 39.0 g/10 minAverage value: 15.7 g/10 min Grade Count:21
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 75.0 - 90.075.0 - 90.0Average value: 82.8 Grade Count:17
Tensile Strength, Ultimate 34.5 - 91.0 MPa5000 - 13200 psiAverage value: 59.8 MPa Grade Count:26
Tensile Strength, Yield 43.0 - 75.2 MPa6240 - 10900 psiAverage value: 55.2 MPa Grade Count:18
Elongation at Break 2.50 - 25.0 %2.50 - 25.0 %Average value: 9.41 % Grade Count:32
Elongation at Yield 4.00 - 9.50 %4.00 - 9.50 %Average value: 6.70 % Grade Count:10
Modulus of Elasticity 2.90 - 8.50 GPa420 - 1230 ksiAverage value: 4.42 GPa Grade Count:29
Flexural Yield Strength 68.9 - 181 MPa10000 - 26300 psiAverage value: 103 MPa Grade Count:33
Flexural Modulus 2.55 - 7.35 GPa370 - 1070 ksiAverage value: 4.04 GPa Grade Count:32
Izod Impact, Notched 0.200 - 5.00 J/cm0.375 - 9.37 ft-lb/inAverage value: 0.878 J/cm Grade Count:23
 0.32034 - 0.48051 J/cm
@Temperature -40.0 - 82.2 °C
0.60013 - 0.90019 ft-lb/in
@Temperature -40.0 - 180 °F
Average value: 0.400 J/cm Grade Count:2
Izod Impact, Unnotched 2.67 - 10.7 J/cm5.00 - 20.0 ft-lb/inAverage value: 7.12 J/cm Grade Count:6
Izod Impact, Notched (ISO) 3.00 - 6.30 kJ/m²1.43 - 3.00 ft-lb/in²Average value: 4.93 kJ/m² Grade Count:7
 3.50 - 3.50 kJ/m²
@Temperature -30.0 - -30.0 °C
1.67 - 1.67 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 3.50 kJ/m² Grade Count:1
Charpy Impact Unnotched 2.20 - 9.03 J/cm²10.5 - 43.0 ft-lb/in²Average value: 6.39 J/cm² Grade Count:7
 5.46 - 9.03 J/cm²
@Temperature -30.0 - -30.0 °C
26.0 - 43.0 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 7.26 J/cm² Grade Count:4
Charpy Impact, Notched 0.200 - 0.680 J/cm²0.952 - 3.24 ft-lb/in²Average value: 0.410 J/cm² Grade Count:24
 0.294 - 0.550 J/cm²
@Temperature -30.0 - -30.0 °C
1.40 - 2.62 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 0.405 J/cm² Grade Count:10
Coefficient of Friction 0.210 - 0.5400.210 - 0.540Average value: 0.420 Grade Count:6
K (wear) Factor 1.00 - 9000 x 10-8 mm³/N-M0.496 - 4470 x 10-10 in³-min/ft-lb-hrAverage value: 3030 x 10-8 mm³/N-M Grade Count:5
Taber Abrasion, mg/1000 Cycles 19.0 - 33.019.0 - 33.0Average value: 27.3 Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+12 - 3.00e+14 ohm-cm1.00e+12 - 3.00e+14 ohm-cmAverage value: 1.24e+14 ohm-cm Grade Count:23
Surface Resistance 1.00e+12 - 7.00e+16 ohm1.00e+12 - 7.00e+16 ohmAverage value: 9.50e+15 ohm Grade Count:19
Dielectric Constant 3.70 - 4.203.70 - 4.20Average value: 3.98 Grade Count:8
Dielectric Strength 19.0 - 86.6 kV/mm483 - 2200 kV/inAverage value: 37.9 kV/mm Grade Count:14
Dissipation Factor 0.00250 - 0.008000.00250 - 0.00800Average value: 0.00565 Grade Count:8
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 - 110 µm/m-°C22.2 - 61.1 µin/in-°FAverage value: 79.7 µm/m-°C Grade Count:24
CTE, linear, Transverse to Flow 80.0 - 120 µm/m-°C44.4 - 66.7 µin/in-°FAverage value: 96.7 µm/m-°C Grade Count:14
Melting Point 160 - 170 °C320 - 338 °FAverage value: 166 °C Grade Count:18
Deflection Temperature at 0.46 MPa (66 psi) 152 - 165 °C306 - 329 °FAverage value: 160 °C Grade Count:16
Deflection Temperature at 1.8 MPa (264 psi) 93.3 - 160 °C200 - 320 °FAverage value: 120 °C Grade Count:36
Vicat Softening Point 155 - 158 °C311 - 316 °FAverage value: 156 °C Grade Count:3
Flammability, UL94 HBHBGrade Count:26
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 230 °C176 - 446 °FAverage value: 167 °C Grade Count:9
Nozzle Temperature 175 - 220 °C347 - 428 °FAverage value: 204 °C Grade Count:5
Die Temperature 190 - 200 °C374 - 392 °FAverage value: 195 °C Grade Count:4
Melt Temperature 120 - 230 °C248 - 446 °FAverage value: 195 °C Grade Count:17
Mold Temperature 60.0 - 120 °C140 - 248 °FAverage value: 91.7 °C Grade Count:17
Drying Temperature 75.0 - 121 °C167 - 250 °FAverage value: 100 °C Grade Count:16
Moisture Content 0.150 - 0.200 %0.150 - 0.200 %Average value: 0.163 % Grade Count:4
Dew Point -31.7 °C-25.0 °FAverage value: -31.7 °C Grade Count:3
Injection Pressure 3.50 - 120 MPa508 - 17400 psiAverage value: 72.2 MPa Grade Count:16

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acetal Copolymer, Impact Modified
Overview of materials for Acetal Copolymer, PTFE Filled
Overview of materials for Acetal Copolymer, Silicone Filled
Overview of materials for Acetal Homopolymer, Unreinforced
Overview of materials for Acetal Copolymer, 20% Glass Fiber Reinforced

O1258 / 77847

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.