MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celanex® 3216 PBT, 15% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: Celanex 3216 is a non-exuding (UL and CSA approved V-0 at 1/32 inch and 5V at 1/8 inch ),15% fiberglass reinforced polybutylene terephthalate which has an excellent balance of mechanical properties and processability. It is well suited for electrical connector applications where its UL approved 50% regrind use capability allows maximum use of purchased product.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.54 g/cc1.54 g/ccASTM D792
Density 1.54 g/cc0.0556 lb/in³ISO 1183
Water Absorption 0.050 %
@Temperature 22.8 °C
0.050 %
@Temperature 73.0 °F
24hr immersion; ASTM D570
Moisture Absorption 0.170 %0.170 %23°C/50%RH; ISO 62
Linear Mold Shrinkage, Flow 0.0030 - 0.0060 cm/cm0.0030 - 0.0060 in/inISO 294-4
 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.011 cm/cm0.011 in/inISO 294-4
Melt Flow 9.0 g/10 min
@Load 2.16 kg,
Temperature 250 °C
9.0 g/10 min
@Load 4.76 lb,
Temperature 482 °F
[cm3/10min]; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8787ISO 2039-2
Tensile Strength at Break 100 MPa14500 psiASTM D638
 100 MPa14500 psi5mm/min; ISO 527-2/1A
Elongation at Break 3.0 %3.0 %5mm/min; ISO 527-2/1A
 4.0 %4.0 %ASTM D638
Tensile Modulus 6.70 GPa972 ksi50mm/min; ISO 527-2/1A
Flexural Strength 152 MPa22000 psiASTM D790
 155 MPa22500 psiISO 178
Flexural Modulus 6.00 GPa870 ksiISO 178
 6.21 GPa900 ksiASTM D790
Izod Impact, Notched 0.534 J/cm1.00 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 5.50 kJ/m²2.62 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched 2.80 J/cm²13.3 ft-lb/in²ISO 179/1eU
 2.80 J/cm²
@Temperature -30.0 °C
13.3 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
 2.00e+16 ohm-cm2.00e+16 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
 3.7
@Frequency 100 Hz
3.7
@Frequency 100 Hz
IEC 60250
Dielectric Strength 26.4 kV/mm670 kV/inshort term; ASTM D149
 30.0 kV/mm762 kV/inIEC 60243-1
Dissipation Factor  0.0033
@Frequency 100 Hz
0.0033
@Frequency 100 Hz
IEC 60250
 0.010
@Frequency 1e+6 Hz
0.010
@Frequency 1e+6 Hz
ASTM D150
 0.016
@Frequency 1e+6 Hz
0.016
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 79 sec79 secASTM D495
Comparative Tracking Index 250 V250 VASTM D3638
 250 V250 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 36.0 µm/m-°C20.0 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°C55.6 µin/in-°FISO 11359-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1,-2,-3
 225 °C437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 213 °C415 °FASTM D648
 217 °C423 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 185 °C365 °FASTM D648
 200 °C392 °FISO 75-1, -2
Deflection Temperature at 8.0 MPa 95.0 °C203 °FISO 75-1, -2
Vicat Softening Point 206 °C403 °FISO 306
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-1,-2,-3
Flammability, UL94 V-0V-0
 5VA
@Thickness 3.00 mm
5VA
@Thickness 0.118 in
Oxygen Index 27 - 32 %27 - 32 %
 
Processing PropertiesMetricEnglishComments
Processing Temperature 65.0 - 93.0 °C149 - 199 °Fcavity
 250 - 260 °C482 - 500 °Fhot runner
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 255 °C464 - 491 °F
Die Temperature 250 - 255 °C482 - 491 °F
Melt Temperature 235 - 255 °C455 - 491 °F
 260 °C500 °FISO 294
Mold Temperature 82.0 °C180 °FISO 294
Injection Velocity 300 mm/sec11.8 in/secISO 294
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4.00 hour4.00 hour
Moisture Content <= 0.020 %<= 0.020 %
Hold Pressure 48.0 MPa6960 psiISO 294
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Polyplastics Duranex® 3216 Polybutylene Terephthalate (PBT), Standard, FR, UL approved regrind 50%, 15% GF filled
Celanese Celanex® 3116 PBT, 7.5% Glass Reinforced
Celanese Celanex® 3100-2 PBT, 7.5% Glass Reinforced
Celanese Celanex® 2016 PBT, Unfilled
Celanese Celanex® 3316 PBT, 30% Glass Reinforced

PHCQ044 / 178499

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.