MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

HP Alloys Alloy X, 30% Cold Worked
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: 30% Cold Worked applies to tensile and/or hardness; other properties are typical of this alloy.

Data provided by High Performance Alloys, Inc., Allvac, and Haynes International.

Key Words: UNS N06002, AMS 5536, AMS 5588, AMS 5754, AMS 5798, AMS 5799, AMS 5888
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.22 g/cc0.297 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1110 MPa161000 psi
Tensile Strength, Yield 945 MPa137000 psi
Elongation at Break 7.0 %7.0 %
Modulus of Elasticity 205 GPa29700 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.0 µm/m-°C
@Temperature 20.0 - 500 °C
8.33 µin/in-°F
@Temperature 68.0 - 932 °F
 16.6 µm/m-°C
@Temperature 20.0 - 1000 °C
9.22 µin/in-°F
@Temperature 68.0 - 1830 °F
Thermal Conductivity 16.9 W/m-K
@Temperature 400 °C
117 BTU-in/hr-ft²-°F
@Temperature 752 °F
Melting Point 1260 - 1355 °C2300 - 2471 °F
Solidus 1260 °C2300 °F
Liquidus 1355 °C2471 °F
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 0.0080 %<= 0.0080 %
Carbon, C 0.10 %0.10 %
Chromium, Cr 22 %22 %
Cobalt, Co 1.5 %1.5 %
Iron, Fe 18 %18 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 9.0 %9.0 %
Nickel, Ni 47 %47 %
Silicon, Si <= 1.0 %<= 1.0 %
Tungsten, W 0.60 %0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Nickelvac® H-X Nickel Superalloy, Heat Treatment: 1177°C (2150°F) Anneal
Haynes Hastelloy® X alloy, sheet
HP Alloys Alloy X, 15% Cold Worked
Special Metals INCONEL® Alloy HX
HP Alloys Alloy X, 5% Cold Worked

NPHX02 / 18809

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.