MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik 11R51 Strip steel
Categories: Metal; Ferrous Metal; Austenitic

Material Notes: Sandvik 11R51 is an austenitic stainless steel with excellent spring properties that in most cases fulfill demands regarding corrosion resistance, mechanical strength, fatigue and relaxation properties. Compared with the standard grade Sandvik 12R11, Sandvik 11R51 offers:
  • Higher tensile strength and tempering effect
  • Higher relaxation resistance, especially at elevated temperatures
  • Higher fatigue strength
  • Better corrosion resistance, due to the addition of molybdenum
Service temperature: up to 300°C (570°F)

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.90 g/cc0.285 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1700 - 2050 MPa247000 - 297000 psiCold rolled
 1900 - 2300 MPa276000 - 334000 psiCold rolled and tempered
Tensile Strength, Yield 1600 - 1975 MPa
@Strain 0.2 %
232000 - 286500 psi
@Strain 0.2 %
Cold rolled
Elongation at Break 0.50 - 1.0 %0.50 - 1.0 %Cold rolled
Modulus of Elasticity 185 GPa26800 ksias delivered
 190 GPa27600 ksitempered
Poissons Ratio 0.300.30as delivered; Calculated
 0.340.34Tempered; Calculated
Shear Modulus 71.0 GPa10300 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.0 µm/m-°C
@Temperature 20.0 - 100 °C
8.33 µin/in-°F
@Temperature 68.0 - 212 °F
 15.5 µm/m-°C
@Temperature 20.0 - 200 °C
8.61 µin/in-°F
@Temperature 68.0 - 392 °F
 16.0 µm/m-°C
@Temperature 20.0 - 300 °C
8.89 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.500 J/g-°C
@Temperature 50.0 - 100 °C
0.120 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity  15.0 W/m-K
@Temperature 20.0 °C
104 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 15.0 W/m-K
@Temperature 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 212 °F
 19.0 W/m-K
@Temperature 300 °C
132 BTU-in/hr-ft²-°F
@Temperature 572 °F
Maximum Service Temperature, Air 300 °C572 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.10 %0.10 %
Chromium, Cr 16.5 %16.5 %
Manganese, Mn 1.2 %1.2 %
Molybdenum, Mo 0.70 %0.70 %
Nickel, Ni 6.5 %6.5 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si 1.2 %1.2 %
Sulfur, S <= 0.010 %<= 0.010 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Eagle Brass 301 Austenitic Stainless Steel, Full Hardened
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
Special Metals DURANICKEL® 301 (UNS N03301) Spring Strip
303 Stainless Steel, annealed
AISI 1018 Steel, as cold drawn, 16-22 mm (0.625-0.875 in) round

NSANDV5061 / 199625

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.