MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Avient Bergamid™ A700 Polyamide 66 (Nylon 66), DAM
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes:

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³±0.02 g/cm³; DIN 53479
Moisture Absorption 2.8 %2.8 %23C/50RH; ISO 62
Water Absorption at Saturation 8.5 %8.5 %ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 80.0 MPa
@Temperature 23.0 °C
11600 psi
@Temperature 73.4 °F
dry as molded; ISO 527-2/50
Elongation at Yield 4.5 %
@Temperature 23.0 °C
4.5 %
@Temperature 73.4 °F
dry as molded; ISO 527-2/50
Tensile Modulus 3.20 GPa
@Temperature 23.0 °C
464 ksi
@Temperature 73.4 °F
dry as molded; ISO 527-2/1
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.600 J/cm²
@Temperature 23.0 °C
2.86 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Constant 3.6
@Frequency 1e+6 Hz
3.6
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 120 kV/mm3050 kV/inIEC 60243-1
Dissipation Factor 0.026
@Frequency 1e+6 Hz
0.026
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VSolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 261 °C502 °FISO 3146
Maximum Service Temperature, Air 90.0 °C194 °FContinuous (GTP 50% Tensile); IEC 60216
 200 °C392 °FShort Time; IEC 60216
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C176 °FUnannealed; ISO 75-2/A
Flammability, UL94 V-2
@Thickness 0.800 mm
V-2
@Thickness 0.0315 in
UL 94
Glow Wire Ignition Temperature 650 °C
@Thickness 0.800 mm
1200 °F
@Thickness 0.0315 in
uncolored material; IEC 60695-2-13
Glow Wire Flammability Index 750 °C
@Thickness 0.800 mm
1380 °F
@Thickness 0.0315 in
Flammability Index; uncolored material; IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 270 - 290 °C518 - 554 °F
Mold Temperature 40.0 - 80.0 °C104 - 176 °F
Drying Temperature 80.0 °C176 °F
Dry Time 4.00 - 8.00 hour4.00 - 8.00 hourDesiccant Dryer
Back Pressure 50.0 - 100 MPa7250 - 14500 psi
 
Descriptive Properties
FormsPellets
Generic MaterialNylon 66
Generic NamePolyamide 66 (Nylon 66)
Processing MethodExtrusion
 Injection Molding
Regional AvailabilityAsia Pacific
 Europe
 North America
RoHS ComplianceRoHS Compliant
UL File NumberE76261Global

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior Akulon® S223-D PA66, Dry
BASF Ultramid® 1000-11 NF2001 PA66 (Dry)
Overview of materials for Polycarbonate, Molded
Overview of materials for Polypropylene, Molded
Celanese Zytel® 101 NC010 PA66

PH0POL0773 / 145342

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.