MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Crastin® FR684NH NC010 PBT-GF25FR(40)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled; Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant

Material Notes: 25% Glass Reinforced, Flame Retardant, Non-Halogenated, Polybutylene Terephthalate

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.52 g/cc0.0549 lb/in³ISO 1183
Water Absorption 0.25 %
@Thickness 2.00 mm
0.25 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.100 %
@Thickness 2.00 mm
0.100 %
@Thickness 0.0787 in
Sim. to ISO 62
Viscosity 150 cP
@Shear Rate 1000 1/s,
Temperature 250 °C
150 cP
@Shear Rate 1000 1/s,
Temperature 482 °F
Melt; ISO 11443
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.011 cm/cm0.011 in/inISO 294-4, 2577
Melt Flow 10 g/10 min
@Load 2.16 kg,
Temperature 250 °C
10 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 100 MPa14500 psiISO 527-1/-2
Elongation at Break 2.7 %2.7 %ISO 527-1/-2
Tensile Modulus 9.40 GPa1360 ksiISO 527-1/-2
Charpy Impact Unnotched 4.70 J/cm²
@Temperature 23.0 °C
22.4 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.790 J/cm²
@Temperature 23.0 °C
3.76 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 44.0 kV/mm1120 kV/inIEC 60243-1
Comparative Tracking Index 500 V500 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 22.0 µm/m-°C12.2 µin/in-°FISO 11359-1/-2
 16.0 µm/m-°C
@Temperature 55.0 - 160 °C
8.89 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
 24.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
13.3 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 120 µm/m-°C66.7 µin/in-°FISO 11359-1/-2
 70.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
 140 µm/m-°C
@Temperature 55.0 - 160 °C
77.8 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
Melting Point 223 °C433 °F10°C/min; ISO 11357-1/-3
 223 °C433 °F10°C/min; ISO 11357-1/-3
 223 °C433 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FISO 75-1/-2
Flammability, UL94  V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
IEC 60695-11-10
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 °C482 °FInjection Optimum
 240 - 260 °C464 - 500 °FInjection
 250 °C482 °FInjection Optimum
 240 - 260 °C464 - 500 °FInjection
 <= 260 °C<= 500 °FInjection
Mold Temperature 30.0 - 130 °C86.0 - 266 °FInjection
 80.0 °C176 °FInjection Optimum
 30.0 - 130 °C86.0 - 266 °FInjection
 80.0 °C176 °FInjection Optimum
 <= 130 °C<= 266 °FInjection
Ejection Temperature 170 °C338 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.040 %0.040 %Injection
Hold Pressure 60.0 MPa8700 psiInjection
 
Descriptive Properties
Back pressureAs low as possibleInjection
Delivery formPellets
Drying RecommendedyesInjection
FMVSS ClassDNIISO 3795 (FMVSS 302)
Hold pressure time (s/mm)3Injection
Part Marking CodePBT-GF25FR(40)ISO 11469
ProcessingInjection Molding
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPBT-GF25FR(40)ISO 1043
Rheological Flow length300 mm80 MPa and 2 mm width/thickness

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Crastin® FR684NH BK591 PBT-GF25FR(40)
Celanese Crastin® HR5315HFS NC010 PBT-IGF15
Envalior Pocan® BFN 4211 000000 PBT, 13% Glass Fiber Reinforced
Envalior Pocan® BFN 4231 000000 PBT, 25% Glass Fiber Reinforced
Celanese Crastin® CE15330 NC010 PBT-GF30FR(17)

PZDSX5016f / 230531

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.