MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Avient Edgetek® NN-50GF/000EM L Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes:

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.57 g/cc1.57 g/ccASTM D792
Water Absorption 0.50 %0.50 %@ 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 121121ASTM D785
Tensile Strength at Break 224 MPa32500 psiType I, 5.1 mm/min; ASTM D638
Elongation at Break 2.0 %2.0 %Type I, 5.1 mm/min; ASTM D638
Tensile Modulus 16.5 GPa2390 ksiType I, 5.1 mm/min; ASTM D638
Flexural Strength 317 MPa46000 psiASTM D790
Flexural Modulus 15.2 GPa2200 ksiASTM D790
Compressive Strength 185 MPa26800 psiASTM D695
Izod Impact, Notched 1.40 J/cm
@Thickness 6.35 mm,
Temperature 23.0 °C
2.62 ft-lb/in
@Thickness 0.250 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 31.0 µm/m-°C17.2 µin/in-°FASTM D696
Thermal Conductivity 0.530 W/m-K3.68 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 254 °C
@Thickness 3.18 mm
489 °F
@Thickness 0.125 in
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 254 °C
@Thickness 3.18 mm
489 °F
@Thickness 0.125 in
Annealed; ASTM D648
Flammability, UL94 HBHBUL 94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 282 - 299 °C540 - 570 °F
Mold Temperature 87.8 - 107 °C190 - 225 °F
Drying Temperature 82.2 - 93.3 °C180 - 200 °F
Dry Time 2.00 hour2.00 hour
 
Descriptive Properties
AdditiveLubricant
 Mold Release
FeaturesLubricated
Filler / ReinforcementGlass Fiber Reinforcement
FormsPellets
Generic MaterialNylon 66
Generic NamePolyamide 66 (Nylon 66)
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Edgetek® NN-50GF/000 Polyamide 66 (Nylon 66)
Avient Edgetek® NN-50GF/000EM Nylon 6/6, Glass Filled
Avient Edgetek® NN-30GF/000 BLACK Nylon 6/6 - 30% Glass Fiber Reinforced
A. Schulman SCHULAMID® 66 GF50H 50% Glass Fiber Reinforced, Heat Stabilized 66
A. Schulman SCHULAMID® 66 GF50 50% Glass Fiber Reinforced 66

PH0POL0686 / 145255

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.