Mid-Mountain Materials CERMEX® PR2200SW Thermal Insulation Mat
Categories:
Ceramic
;
Glass
;
Glass Fiber
;
Oxide
;
Silicon Oxide
;
Other Engineering Material
;
Composite Fibers
Material Notes:
Material: Alkaline Earth Silicate Wool
Construction: Paper, Organic Binder
Information provided by Mid-Mountain Materials
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
0.176
-
0.224
g/cc
0.00637
-
0.00810
lb/in³
Loss On Ignition
5.0 - 10 %
5.0 - 10 %
Thickness
3125
microns
123.0
mil
6250
microns
246
mil
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
0.0345
-
0.0689
MPa
5.00
-
10.0
psi
Fired Material
0.414
-
0.621
MPa
60.0
-
90.0
psi
Standard Material
Thermal Properties
Metric
English
Comments
Thermal Conductivity
0.0600
W/m-K
@Temperature 260 °C
0.416
BTU-in/hr-ft²-°F
@Temperature 500 °F
0.0900
W/m-K
@Temperature 538 °C
0.625
BTU-in/hr-ft²-°F
@Temperature 1000 °F
0.150
W/m-K
@Temperature 816 °C
1.04
BTU-in/hr-ft²-°F
@Temperature 1500 °F
0.220
W/m-K
@Temperature 1093 °C
1.53
BTU-in/hr-ft²-°F
@Temperature 1999 °F
Melting Point
>=
1300
°C
>=
2370
°F
Maximum Service Temperature, Air
1200
°C
2200
°F
Continuous
1260
°C
2300
°F
Intermittent
Component Elements Properties
Metric
English
Comments
CaO
16 - 22 %
16 - 22 %
MgO
12 - 19 %
12 - 19 %
Other
<= 1.0 %
<= 1.0 %
SiO2
60 - 70 %
60 - 70 %
Descriptive Properties
Al
2
O
3
(%)
Trace
Color
White
Fiber Index (%)
60
Width (in)
12
24
48
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Parabeam Industrie Paraglass 3 3D Glass Fabric
Pyrotek Firefly 800 Roller & Furnace Cladding Material
3M Scotchcast™ 2123 Re-enterable Insulating Electrical Resin
Mid-Mountain Materials CERMEX® PR1800SW Low Biopersistence Thermal Insulation Paper
Avient Versaflex™ CL2003X Thermoplastic Elastomer (TPE)
CMID70 / 141238
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.