MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik 316L Plate and Sheet
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Sandvik 316L is a molybdenum alloyed austenitic stainless chromium nickel steel with a low carbon content.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell <= 95<= 95
Tensile Strength, Ultimate 485 MPa70300 psi
Tensile Strength, Yield  >= 170 MPa
@Strain 0.2 %
>= 24700 psi
@Strain 0.2 %
 >= 250 MPa
@Strain 1 %
>= 36300 psi
@Strain 1 %
 >= 110 MPa
@Strain 0.2 %,
Temperature 600 °C
>= 16000 psi
@Strain 0.2 %,
Temperature 1110 °F
 >= 115 MPa
@Strain 0.2 %,
Temperature 550 °C
>= 16700 psi
@Strain 0.2 %,
Temperature 1020 °F
 >= 120 MPa
@Strain 0.2 %,
Temperature 450 °C
>= 17400 psi
@Strain 0.2 %,
Temperature 842 °F
 >= 120 MPa
@Strain 0.2 %,
Temperature 500 °C
>= 17400 psi
@Strain 0.2 %,
Temperature 932 °F
 >= 125 MPa
@Strain 0.2 %,
Temperature 400 °C
>= 18100 psi
@Strain 0.2 %,
Temperature 752 °F
 >= 130 MPa
@Strain 0.2 %,
Temperature 350 °C
>= 18900 psi
@Strain 0.2 %,
Temperature 662 °F
 >= 135 MPa
@Strain 0.2 %,
Temperature 300 °C
>= 19600 psi
@Strain 0.2 %,
Temperature 572 °F
 >= 135 MPa
@Strain 1 %,
Temperature 600 °C
>= 19600 psi
@Strain 1 %,
Temperature 1110 °F
 >= 140 MPa
@Strain 1 %,
Temperature 550 °C
>= 20300 psi
@Strain 1 %,
Temperature 1020 °F
 >= 140 MPa
@Strain 0.2 %,
Temperature 250 °C
>= 20300 psi
@Strain 0.2 %,
Temperature 482 °F
 >= 145 MPa
@Strain 1 %,
Temperature 450 °C
>= 21000 psi
@Strain 1 %,
Temperature 842 °F
 >= 145 MPa
@Strain 1 %,
Temperature 500 °C
>= 21000 psi
@Strain 1 %,
Temperature 932 °F
 >= 150 MPa
@Strain 1 %,
Temperature 400 °C
>= 21800 psi
@Strain 1 %,
Temperature 752 °F
 >= 150 MPa
@Strain 0.2 %,
Temperature 200 °C
>= 21800 psi
@Strain 0.2 %,
Temperature 392 °F
 >= 155 MPa
@Strain 1 %,
Temperature 350 °C
>= 22500 psi
@Strain 1 %,
Temperature 662 °F
 >= 160 MPa
@Strain 1 %,
Temperature 300 °C
>= 23200 psi
@Strain 1 %,
Temperature 572 °F
 >= 165 MPa
@Strain 0.2 %,
Temperature 150 °C
>= 23900 psi
@Strain 0.2 %,
Temperature 302 °F
 >= 170 MPa
@Strain 1 %,
Temperature 250 °C
>= 24700 psi
@Strain 1 %,
Temperature 482 °F
 >= 180 MPa
@Strain 0.2 %,
Temperature 100 °C
>= 26100 psi
@Strain 0.2 %,
Temperature 212 °F
 >= 180 MPa
@Strain 1 %,
Temperature 200 °C
>= 26100 psi
@Strain 1 %,
Temperature 392 °F
 >= 195 MPa
@Strain 1 %,
Temperature 150 °C
>= 28300 psi
@Strain 1 %,
Temperature 302 °F
 >= 200 MPa
@Strain 0.2 %,
Temperature 50.0 °C
>= 29000 psi
@Strain 0.2 %,
Temperature 122 °F
 >= 215 MPa
@Strain 1 %,
Temperature 100 °C
>= 31200 psi
@Strain 1 %,
Temperature 212 °F
 >= 230 MPa
@Strain 1 %,
Temperature 50.0 °C
>= 33400 psi
@Strain 1 %,
Temperature 122 °F
Elongation at Break >= 35 %>= 35 %
 >= 40 %>= 40 %Based on L = 5.65 ÖS where L is the original gauge length and S the original cross section area.
Creep Strength  18.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
2610 psi
@Temperature 1380 °F,
Time 100000 hour
 25.0 MPa
@Temperature 725 °C,
Time 3.60e+8 sec
3630 psi
@Temperature 1340 °F,
Time 100000 hour
 33.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
4790 psi
@Temperature 1290 °F,
Time 100000 hour
 37.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
5370 psi
@Temperature 1380 °F,
Time 10000 hour
 46.0 MPa
@Temperature 675 °C,
Time 3.60e+8 sec
6670 psi
@Temperature 1250 °F,
Time 100000 hour
 49.0 MPa
@Temperature 725 °C,
Time 3.60e+7 sec
7110 psi
@Temperature 1340 °F,
Time 10000 hour
 64.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
9280 psi
@Temperature 1290 °F,
Time 10000 hour
 64.0 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
9280 psi
@Temperature 1200 °F,
Time 100000 hour
 83.0 MPa
@Temperature 675 °C,
Time 3.60e+7 sec
12000 psi
@Temperature 1250 °F,
Time 10000 hour
 86.0 MPa
@Temperature 625 °C,
Time 3.60e+8 sec
12500 psi
@Temperature 1160 °F,
Time 100000 hour
 108 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
15700 psi
@Temperature 1200 °F,
Time 10000 hour
 108 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
15700 psi
@Temperature 1110 °F,
Time 100000 hour
 137 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
19900 psi
@Temperature 1070 °F,
Time 100000 hour
 137 MPa
@Temperature 625 °C,
Time 3.60e+7 sec
19900 psi
@Temperature 1160 °F,
Time 10000 hour
 172 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
24900 psi
@Temperature 1110 °F,
Time 10000 hour
 177 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
25700 psi
@Temperature 1020 °F,
Time 100000 hour
 214 MPa
@Temperature 575 °C,
Time 3.60e+7 sec
31000 psi
@Temperature 1070 °F,
Time 10000 hour
 255 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
37000 psi
@Temperature 1020 °F,
Time 10000 hour
Modulus of Elasticity  165 GPa
@Temperature 500 °C
23900 ksi
@Temperature 932 °F
 172 GPa
@Temperature 400 °C
24900 ksi
@Temperature 752 °F
 179 GPa
@Temperature 300 °C
26000 ksi
@Temperature 572 °F
 186 GPa
@Temperature 200 °C
27000 ksi
@Temperature 392 °F
 194 GPa
@Temperature 100 °C
28100 ksi
@Temperature 212 °F
 200 GPa
@Temperature 20.0 °C
29000 ksi
@Temperature 68.0 °F
Charpy Impact 150 J
@Temperature -60.0 °C
111 ft-lb
@Temperature -76.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.5 µm/m-°C
@Temperature 30.0 - 100 °C
9.17 µin/in-°F
@Temperature 86.0 - 212 °F
 17.0 µm/m-°C
@Temperature 30.0 - 200 °C
9.44 µin/in-°F
@Temperature 86.0 - 392 °F
 17.5 µm/m-°C
@Temperature 30.0 - 300 °C
9.72 µin/in-°F
@Temperature 86.0 - 572 °F
 18.0 µm/m-°C
@Temperature 30.0 - 400 °C
10.0 µin/in-°F
@Temperature 86.0 - 752 °F
 18.0 µm/m-°C
@Temperature 30.0 - 500 °C
10.0 µin/in-°F
@Temperature 86.0 - 932 °F
 18.5 µm/m-°C
@Temperature 30.0 - 600 °C
10.3 µin/in-°F
@Temperature 86.0 - 1110 °F
 18.5 µm/m-°C
@Temperature 30.0 - 700 °C
10.3 µin/in-°F
@Temperature 86.0 - 1290 °F
Specific Heat Capacity  0.500 J/g-°C
@Temperature 100 °C
0.120 BTU/lb-°F
@Temperature 212 °F
 0.515 J/g-°C
@Temperature 200 °C
0.123 BTU/lb-°F
@Temperature 392 °F
 0.525 J/g-°C
@Temperature 300 °C
0.125 BTU/lb-°F
@Temperature 572 °F
 0.540 J/g-°C
@Temperature 400 °C
0.129 BTU/lb-°F
@Temperature 752 °F
 0.555 J/g-°C
@Temperature 500 °C
0.133 BTU/lb-°F
@Temperature 932 °F
 0.575 J/g-°C
@Temperature 600 °C
0.137 BTU/lb-°F
@Temperature 1110 °F
 0.850 J/g-°C
@Temperature 20.0 °C
0.203 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity  14.0 W/m-K
@Temperature 20.0 °C
97.2 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 15.0 W/m-K
@Temperature 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 212 °F
 17.0 W/m-K
@Temperature 200 °C
118 BTU-in/hr-ft²-°F
@Temperature 392 °F
 18.0 W/m-K
@Temperature 300 °C
125 BTU-in/hr-ft²-°F
@Temperature 572 °F
 20.0 W/m-K
@Temperature 400 °C
139 BTU-in/hr-ft²-°F
@Temperature 752 °F
 21.0 W/m-K
@Temperature 500 °C
146 BTU-in/hr-ft²-°F
@Temperature 932 °F
 23.0 W/m-K
@Temperature 600 °C
160 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.030 %0.030 %
Chromium, Cr 16 - 18 %16 - 18 %
Manganese, Mn 2.0 %2.0 %
Molybdenum, Mo 2.0 - 3.0 %2.0 - 3.0 %
Nickel, Ni 10 - 14 %10 - 14 %
Nitrogen, N 0.10 %0.10 %
Phosphorus, P 0.045 %0.045 %
Silicon, Si 0.75 %0.75 %
Sulfur, S 0.030 %0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 316L Stainless Steel, annealed sheet
Eagle Brass 316L Austenitic Stainless Steel, Full Hardened
AISI Type 316L Stainless Steel, annealed plate
Outokumpu 253MA® High Temperature Austenitic Stainless Steel
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Annealed

NSANDV5151 / 199715

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.