MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Zinc AC41A Alloy (Zamak 5), As Cast
Categories: Metal; Nonferrous Metal; Zinc Alloy

Material Notes: The composition listed is according to ASTM B86 specifications. Conflicting sources on composition. One source gives Mg content as 0.020 - 0.05% with a footnote saying the Mg content can be as low as 0.015% as long as the Pb, Cd, and Sn contents do not exceed 0.003, 0.003, and 0.001% respectively. The same source does not list Cu as a constituent of AC41A. Another source lists the Mg content as 0.030 - 0.080%. Suggested Casting Temperature 395-425°C (745-795°F).

Key Words: ASTM C41A; SAE 925; UNS Z35530 (ingot), UNS Z35531 (casting); ASTM B240; ASTM B86, Mazak 5, Zamac5
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 6.70 g/cc0.242 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 9191500 kg load; 10 mm hardened steel ball
Hardness, Knoop 115115Estimated from Brinell Hardness
Hardness, Rockwell A 3838Estimated from Brinell Hardness
Hardness, Rockwell B 5757Estimated from Brinell Hardness
Hardness, Vickers 102102Estimated from Brinell Hardness
Tensile Strength, Ultimate 330 MPa47900 psi
Elongation at Break 7.0 %7.0 %in 50 mm
Compressive Strength 600 MPa87000 psi
Fatigue Strength 56.5 MPa
@# of Cycles 5.00e+8
8190 psi
@# of Cycles 5.00e+8
Reverse Bending
Shear Strength 260 MPa37700 psi
Charpy Impact, Unnotched 65.0 J47.9 ft-lb6.4 mm x 6.4 mm bar
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000650 ohm-cm0.00000650 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 27.4 µm/m-°C
@Temperature 20.0 °C
15.2 µin/in-°F
@Temperature 68.0 °F
Specific Heat Capacity 0.420 J/g-°C0.100 BTU/lb-°F
Thermal Conductivity 109 W/m-K756 BTU-in/hr-ft²-°F
Melting Point 380 - 386 °C716 - 727 °F
Solidus 380 °C716 °F
Liquidus 386 °C727 °F
 
Processing PropertiesMetricEnglishComments
Casting Temperature 395 - 425 °C743 - 797 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.5 - 4.3 %3.5 - 4.3 %Casting
 3.9 - 4.3 %3.9 - 4.3 %Ingot form
Cadmium, Cd <= 0.0030 %<= 0.0030 %Ingot form
 <= 0.0040 %<= 0.0040 %Casting
Copper, Cu 0.75 - 1.25 %0.75 - 1.25 %Casting
 0.75 - 1.25 %0.75 - 1.25 %Ingot form
Iron, Fe <= 0.075 %<= 0.075 %Ingot form
 <= 0.10 %<= 0.10 %Casting
Lead, Pb <= 0.0040 %<= 0.0040 %Ingot form
 <= 0.0050 %<= 0.0050 %Casting
Magnesium, Mg 0.030 - 0.060 %0.030 - 0.060 %Ingot form
 0.030 - 0.080 %0.030 - 0.080 %Casting
Tin, Sn <= 0.0020 %<= 0.0020 %Ingot form
 <= 0.0030 %<= 0.0030 %Casting
Zinc, Zn 94.306 - 95.32 %94.306 - 95.32 %As balance; Ingot per ASTM B 240
 94.258 - 95.72 %94.258 - 95.72 %As balance; Castings per ASTM B 86

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zinc AG40A (Zinc Alloy 3; Zn-4Al-0.4Mg; Zamak 3), Cast
Zinc AC41A (Zamak 5), Cast and Aged
Zinc AC43A (Zinc Alloy 2; Zn-4Al-2.5Cu-0.04Mg; Number 2 Die Casting Alloy; Zamak 2), Die Cast
Zinc Alloy 7; AG40B; Zn-4Al-0.015Mg; Zamak7
Zinc AG40A (Zinc Alloy 3; Zn-4Al-0.4Mg; Zamak 3), Cast and Aged

MZn41A / 14526

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.