MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

3D Systems LaserForm® AlSi10Mg (A), AS-BUILT Aluminum Alloy Material
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: AlSi10Mg fine-tuned for use with ProX® DMP 320 metal printer producing industrial parts with a combination of good mechanical properties and good thermal conductivity. LaserForm AlSi10Mg (A) is formulated and fine-tuned specifically for 3D Systems DMP 320 metal 3D Printers to deliver high part quality and consistent part properties.

AlSi10Mg combines silicon and magnesium as alloying elements, which results in a significant increase in strength and hardness compared to other aluminum alloys. Due to the very rapid melting and solidification during Direct Metal Printing, LaserForm AlSi10Mg (A) in as-printed condition shows fine microstructure and high strengths. In the aerospace and automotive industry, LaserForm AlSi10Mg (A) is used for its light weight. Both innovative approaches to mold design and specific heat exchanger applications make use of the high thermal conductivity of this alloy.

Information provided by 3D Systems

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.68 g/cc0.0968 lb/in³Absolute theoretical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 67 - 7567 - 75ASTM E18
Tensile Strength, Ultimate 360 - 480 MPa52200 - 69600 psiVertical direction - Z; ASTM E8M
 420 - 480 MPa60900 - 69600 psiHorizontal direction - XY; ASTM E8M
Tensile Strength, Yield 190 - 270 MPa27600 - 39200 psiRp0.2%, Vertical direction - Z; ASTM E8M
 230 - 290 MPa33400 - 42100 psiRp0.2%, Horizontal direction - XY; ASTM E8M
Elongation at Break 3.0 - 7.0 %3.0 - 7.0 %Vertical direction - Z; ASTM E8M
 4.0 - 12 %4.0 - 12 %Horizontal direction - XY; ASTM E8M
Tensile Modulus 6.90 - 7.30 GPa1000 - 1060 ksiYoungs
Charpy Impact 3.00 - 4.00 J2.21 - 2.95 ft-lbNotch; ASTM E23
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.9 µm/m-°C
@Temperature 20.0 - 100 °C
11.6 µin/in-°F
@Temperature 68.0 - 212 °F
Thermal Conductivity 113 W/m-K784 BTU-in/hr-ft²-°F
Melting Point 557 - 596 °C1030 - 1100 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 87.15 - 90.8 %87.15 - 90.8 %Balance
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.55 %<= 0.55 %
Lead, Pb <= 0.050 %<= 0.050 %
Magnesium, Mg 0.20 - 0.45 %0.20 - 0.45 %
Manganese, Mn <= 0.35 %<= 0.35 %
Nickel, Ni <= 0.050 %<= 0.050 %
Silicon, Si 9.0 - 11 %9.0 - 11 %
Tin, Sn <= 0.050 %<= 0.050 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.10 %<= 0.10 %
 
Descriptive Properties
Surface Roughness7-10µmVertical direction (Z), SAND BLASTED

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum A380.0-F Die Casting Alloy
Aluminum 6063-T5
Proto Labs Aluminum AlSi10Mg - DMLS
3D Systems LaserForm® AlSi10Mg (A), DIRECT AGING Aluminum Alloy Material
Aluminum A360.0-F Die Casting Alloy

PAPPR3121 / 239089

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.