MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Liquid Crystal Polymer (LCP), Mineral Filled
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Liquid Crystal Polymer (LCP), Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.52 - 1.89 g/cc0.0549 - 0.0683 lb/in³Average value: 1.70 g/cc Grade Count:32
Filler Content 30.0 - 50.0 %30.0 - 50.0 %Average value: 40.0 % Grade Count:6
Water Absorption 0.0200 - 0.100 %0.0200 - 0.100 %Average value: 0.0380 % Grade Count:10
Moisture Absorption at Equilibrium 0.0200 - 0.0400 %0.0200 - 0.0400 %Average value: 0.0233 % Grade Count:6
Linear Mold Shrinkage 0.000 - 0.00300 cm/cm0.000 - 0.00300 in/inAverage value: 0.00125 cm/cm Grade Count:26
Linear Mold Shrinkage, Transverse 0.00200 - 0.0110 cm/cm0.00200 - 0.0110 in/inAverage value: 0.00568 cm/cm Grade Count:24
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 43.0 - 90.043.0 - 90.0Average value: 65.5 Grade Count:8
Tensile Strength, Ultimate 76.0 - 175 MPa11000 - 25400 psiAverage value: 128 MPa Grade Count:32
 48.0 - 200 MPa
@Temperature -40.0 - 150 °C
6960 - 29000 psi
@Temperature -40.0 - 302 °F
Average value: 86.6 MPa Grade Count:1
 17.0 - 216 MPa
@Temperature -40.0 - 250 °C
2470 - 31300 psi
@Temperature -40.0 - 482 °F
Average value: 86.6 MPa Grade Count:1
 17.0 - 216 MPa
@Thickness 1.60 - 3.17 mm
2470 - 31300 psi
@Thickness 0.0630 - 0.125 in
Average value: 86.6 MPa Grade Count:1
Elongation at Break 1.20 - 5.50 %1.20 - 5.50 %Average value: 3.35 % Grade Count:30
 2.50 - 3.20 %
@Temperature 120 - 150 °C
2.50 - 3.20 %
@Temperature 248 - 302 °F
Average value: 2.06 % Grade Count:1
 0.700 - 3.20 %
@Temperature -40.0 - 250 °C
0.700 - 3.20 %
@Temperature -40.0 - 482 °F
Average value: 2.06 % Grade Count:1
 0.700 - 3.20 %
@Thickness 1.60 - 3.17 mm
0.700 - 3.20 %
@Thickness 0.0630 - 0.125 in
Average value: 2.06 % Grade Count:1
Modulus of Elasticity 7.03 - 22.0 GPa1020 - 3190 ksiAverage value: 11.9 GPa Grade Count:27
 4.80 - 11.6 GPa
@Temperature -40.0 - 150 °C
696 - 1680 ksi
@Temperature -40.0 - 302 °F
Average value: 7.45 GPa Grade Count:1
 2.77 - 16.5 GPa
@Temperature -40.0 - 250 °C
402 - 2390 ksi
@Temperature -40.0 - 482 °F
Average value: 7.45 GPa Grade Count:1
 2.77 - 16.5 GPa
@Thickness 1.60 - 3.17 mm
402 - 2390 ksi
@Thickness 0.0630 - 0.125 in
Average value: 7.45 GPa Grade Count:1
Flexural Yield Strength 87.0 - 230 MPa12600 - 33400 psiAverage value: 151 MPa Grade Count:29
 42.0 - 260 MPa
@Temperature -40.0 - 150 °C
6090 - 37700 psi
@Temperature -40.0 - 302 °F
Average value: 109 MPa Grade Count:2
 42.0 - 260 MPa
@Thickness 0.800 - 3.17 mm
6090 - 37700 psi
@Thickness 0.0315 - 0.125 in
Average value: 109 MPa Grade Count:2
Flexural Modulus 6.60 - 20.0 GPa957 - 2900 ksiAverage value: 11.5 GPa Grade Count:32
 3.30 - 16.7 GPa
@Temperature -40.0 - 150 °C
479 - 2420 ksi
@Temperature -40.0 - 302 °F
Average value: 7.38 GPa Grade Count:2
 3.30 - 16.7 GPa
@Thickness 0.800 - 3.17 mm
479 - 2420 ksi
@Thickness 0.0315 - 0.125 in
Average value: 7.38 GPa Grade Count:2
Flexural Strain at Break 2.00 - 2.40 %2.00 - 2.40 %Average value: 2.23 % Grade Count:3
Compressive Yield Strength 51.7 - 131 MPa7500 - 19000 psiAverage value: 81.6 MPa Grade Count:8
Compressive Modulus 9.50 - 21.5 GPa1380 - 3120 ksiAverage value: 14.1 GPa Grade Count:7
Izod Impact, Notched 0.500 - 1.60 J/cm0.937 - 3.00 ft-lb/inAverage value: 0.996 J/cm Grade Count:5
Izod Impact, Notched (ISO) 5.00 - 60.0 kJ/m²2.38 - 28.6 ft-lb/in²Average value: 26.9 kJ/m² Grade Count:12
Charpy Impact Unnotched 2.10 - 8.40 J/cm²9.99 - 40.0 ft-lb/in²Average value: 5.64 J/cm² Grade Count:7
 4.00 - 4.00 J/cm²
@Temperature -30.0 - -30.0 °C
19.0 - 19.0 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 4.00 J/cm² Grade Count:2
Charpy Impact, Notched 0.273 - 4.00 J/cm²1.30 - 19.0 ft-lb/in²Average value: 1.14 J/cm² Grade Count:24
 0.700 - 0.800 J/cm²
@Temperature -30.0 - -30.0 °C
3.33 - 3.81 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 0.750 J/cm² Grade Count:2
Tensile Impact Strength 40.0 - 80.0 kJ/m²19.0 - 38.1 ft-lb/in²Average value: 56.7 kJ/m² Grade Count:3
Coefficient of Friction 0.120 - 0.2100.120 - 0.210Average value: 0.172 Grade Count:4
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+12 - 2.50e+16 ohm-cm1.00e+12 - 2.50e+16 ohm-cmAverage value: 3.86e+15 ohm-cm Grade Count:18
Surface Resistance 3.10e+11 - 1.00e+17 ohm3.10e+11 - 1.00e+17 ohmAverage value: 1.46e+16 ohm Grade Count:17
Dielectric Constant 2.90 - 6.702.90 - 6.70Average value: 3.81 Grade Count:17
 4.00 - 4.20
@Temperature 120 - 250 °C
4.00 - 4.20
@Temperature 248 - 482 °F
Average value: 4.06 Grade Count:2
 4.00 - 4.20
@Frequency 1.00e+9 - 1.00e+10 Hz
4.00 - 4.20
@Frequency 1.00e+9 - 1.00e+10 Hz
Average value: 4.06 Grade Count:2
Dielectric Strength 22.0 - 66.0 kV/mm559 - 1680 kV/inAverage value: 38.1 kV/mm Grade Count:10
Dissipation Factor 5.70e-7 - 0.03405.70e-7 - 0.0340Average value: 0.0128 Grade Count:17
 0.00500 - 0.0290
@Temperature 120 - 250 °C
0.00500 - 0.0290
@Temperature 248 - 482 °F
Average value: 0.0149 Grade Count:2
 0.00500 - 0.0290
@Frequency 1.00e+9 - 1.00e+10 Hz
0.00500 - 0.0290
@Frequency 1.00e+9 - 1.00e+10 Hz
Average value: 0.0149 Grade Count:2
Arc Resistance 145 - 183 sec145 - 183 secAverage value: 174 sec Grade Count:8
Comparative Tracking Index 150 - 250 V150 - 250 VAverage value: 199 V Grade Count:17
 
Thermal PropertiesMetricEnglishComments
CTE, linear -10.0 - 19.8 µm/m-°C-5.56 - 11.0 µin/in-°FAverage value: 6.87 µm/m-°C Grade Count:19
 18.0 - 18.0 µm/m-°C
@Temperature 20.0 - 180 °C
10.0 - 10.0 µin/in-°F
@Temperature 68.0 - 356 °F
Average value: 8.91 µm/m-°C Grade Count:1
 -4.00 - 20.0 µm/m-°C
@Temperature 55.0 - 260 °C
-2.22 - 11.1 µin/in-°F
@Temperature 131 - 500 °F
Average value: 8.91 µm/m-°C Grade Count:3
 -4.00 - 20.0 µm/m-°C
@Thickness 2.00 - 4.00 mm
-2.22 - 11.1 µin/in-°F
@Thickness 0.0787 - 0.157 in
Average value: 8.91 µm/m-°C Grade Count:3
CTE, linear, Transverse to Flow 22.0 - 93.6 µm/m-°C12.2 - 52.0 µin/in-°FAverage value: 44.2 µm/m-°C Grade Count:19
 88.2 - 100.8 µm/m-°C
@Temperature 20.0 - 180 °C
49.0 - 56.00 µin/in-°F
@Temperature 68.0 - 356 °F
Average value: 52.0 µm/m-°C Grade Count:1
 34.0 - 62.0 µm/m-°C
@Temperature 55.0 - 260 °C
18.9 - 34.4 µin/in-°F
@Temperature 131 - 500 °F
Average value: 52.0 µm/m-°C Grade Count:3
 34.0 - 62.0 µm/m-°C
@Thickness 2.00 - 4.00 mm
18.9 - 34.4 µin/in-°F
@Thickness 0.0787 - 0.157 in
Average value: 52.0 µm/m-°C Grade Count:3
Specific Heat Capacity 0.000870 - 0.00138 J/g-°C0.000208 - 0.000330 BTU/lb-°FAverage value: 0.00112 J/g-°C Grade Count:4
Thermal Conductivity 0.476 - 2.45 W/m-K3.30 - 17.0 BTU-in/hr-ft²-°FAverage value: 0.988 W/m-K Grade Count:3
Melting Point 128 - 335 °C262 - 635 °FAverage value: 309 °C Grade Count:25
Maximum Service Temperature, Air 130 °C266 °FAverage value: 130 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 203 - 281 °C397 - 538 °FAverage value: 262 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 185 - 295 °C365 - 563 °FAverage value: 234 °C Grade Count:32
Vicat Softening Point 151 - 238 °C304 - 460 °FAverage value: 208 °C Grade Count:3
Glass Transition Temp, Tg 120 °C248 °FAverage value: 120 °C Grade Count:3
UL RTI, Electrical 130 - 240 °C266 - 464 °FAverage value: 161 °C Grade Count:12
UL RTI, Mechanical with Impact 130 - 220 °C266 - 428 °FAverage value: 156 °C Grade Count:12
UL RTI, Mechanical without Impact 130 - 240 °C266 - 464 °FAverage value: 185 °C Grade Count:6
Flammability, UL94 V-0V-0Grade Count:21
Oxygen Index 40.0 - 47.0 %40.0 - 47.0 %Average value: 43.5 % Grade Count:4
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 345 °C68.0 - 653 °FAverage value: 147 °C Grade Count:7
Nozzle Temperature 320 - 345 °C608 - 653 °FAverage value: 336 °C Grade Count:5
Die Temperature 290 - 360 °C554 - 680 °FAverage value: 333 °C Grade Count:5
Melt Temperature 270 - 399 °C518 - 750 °FAverage value: 334 °C Grade Count:22
Mold Temperature 30.0 - 160 °C86.0 - 320 °FAverage value: 92.5 °C Grade Count:18
Drying Temperature 149 - 170 °C300 - 338 °FAverage value: 151 °C Grade Count:20
Moisture Content 0.0100 %0.0100 %Average value: 0.0100 % Grade Count:12
Dew Point -40.0 - -28.9 °C-40.0 - -20.0 °FAverage value: -32.6 °C Grade Count:3
Injection Pressure 50.0 - 200 MPa7250 - 29000 psiAverage value: 105 MPa Grade Count:11

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Liquid Crystal Polymer (LCP), Unfilled
Overview of materials for Liquid Crystal Polymer (LCP), 20% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled
Overview of materials for Liquid Crystal Polymer (LCP), Carbon Fiber Filled

O2249 / 77950

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.