MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

TSE Industries Millathane® CM Millable Polyether Urethane Rubber, 0.75 PHR Sulfur
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: MILLATHANE CM is a sulfur and peroxide curable polyether urethane rubber. Its outstanding property is its great resistance to abrasion, which makes it of special interest for articles that are subjected to high wear in service. It has a unique combination of excellent properties, such as low temperature characteristics, and resistance to heat deterioration, ozone cracking, weathering and swelling in oils or solvents.

All information provided by TSE Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6565
 6868after 7 days at 100ºC
Tensile Strength 27.9 MPa4050 psiafter 7 days at 100ºC
 31.0 MPa4500 psi
Elongation at Break 390 %390 %after 7 days at 100ºC
 480 %480 %
300% Modulus  14.65 MPa
@Strain 300 %
2125 psi
@Strain 300 %
 19.48 MPa
@Strain 300 %
2825 psi
@Strain 300 %
after 7 days at 100ºC
Abrasion 335335NBS Index
Compression Set 19 %
@Temperature 70.0 °C,
Time 79200 sec
19 %
@Temperature 158 °F,
Time 22.0 hour
Method B
 
Processing PropertiesMetricEnglishComments
Cure Time 60.0 min
@Temperature 142 °C
1.00 hour
@Temperature 287 °F
 
Descriptive Properties
ΔT, Platen (ºC)60
Formulation as Tested0.35CAYTUR 4
 0.75Zinc Stearate
 0.75Sulfur
 1MBT
 100Millathane CM
 15Coumarone-Indene Resin
 30N330 Carbon Black
 4MBTS
Heat Build-up, Internal Temp (ºC)135Goodrich Flexometer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
TSE Industries Millathane® CM Millable Polyether Urethane Rubber, 0.5 PHR Sulfur
TSE Industries Millathane® CM Millable Polyether Urethane Rubber, 1.5 PHR Sulfur
Tra-Con Tra-Sheet BFG Thermally Conductive Sheet
Lubrizol ESTANE® 58881 Ether Based Thermoplastic Polyurethane
Lubrizol ESTANE® 58202 Ether Based Thermoplastic Polyurethane

PMILL140 / 87184

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.