System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
BASF Ultramid® B3GK24 BK 00564 10/20% Glass/Glass Bead Filled PA6 (Conditioned)
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 10% Glass Fiber Filled
;
Nylon 6, Glass Bead Filled
Material Notes:
Description: combined 10% glass-fiber and 20% glass-bead reinforced injection-molding grade for technical articles of very good dimensional stability, for instance, vehicle ash tray housings and electronic housings.
Information provided by BASF
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Bulk Density
0.500
-
0.800
g/cc
0.0181
-
0.0289
lb/in³
Density
1.34
g/cc
0.0484
lb/in³
ISO 1183
Moisture Absorption at Equilibrium
1.9 - 2.3 %
1.9 - 2.3 %
23°C; 50% RH; ISO 62
Water Absorption at Saturation
6.3 - 6.9 %
6.3 - 6.9 %
ISO 62
Viscosity Measurement
140
140
ISO 307
Linear Mold Shrinkage
0.0050
cm/cm
0.0050
in/in
restricted
Melt Flow
93.8
g/10 min
@Load 5.00 kg,
Temperature 275 °C
93.8
g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
60.0
MPa
8700
psi
50 mm/min; ISO 527-1/-2
Elongation at Yield
15 %
15 %
50 mm/min; ISO 527-1/-2
Modulus of Elasticity
3.00
GPa
435
ksi
ISO 527-1/-2
Flexural Strength
70.0
MPa
10200
psi
at max force; ISO 178
100
MPa
14500
psi
ISO 178
Flexural Modulus
3.00
GPa
435
ksi
ISO 178
Izod Impact, Notched (ISO)
8.50
kJ/m²
@Temperature 23.0 °C
4.04
ft-lb/in²
@Temperature 73.4 °F
ISO 180/A
Charpy Impact Unnotched
9.00
J/cm²
@Temperature 23.0 °C
42.8
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched
1.10
J/cm²
@Temperature 23.0 °C
5.23
ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
Tensile Creep Modulus, 1000 hours
2000
MPa
@Strain <=0.5 %
290000
psi
@Strain <=0.5 %
ISO 899-1
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+10
ohm-cm
1.00e+10
ohm-cm
IEC 60093
Surface Resistance
1.00e+10
ohm
1.00e+10
ohm
IEC 60093
Dielectric Constant
4.6
@Frequency 1e+6 Hz
4.6
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor
0.070
@Frequency 1e+6 Hz
0.070
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
425
V
425
V
Test solution A; IEC 60112
Thermal Properties
Metric
English
Comments
Specific Heat Capacity
1.40
J/g-°C
0.335
BTU/lb-°F
Thermal Conductivity
0.340
W/m-K
2.36
BTU-in/hr-ft²-°F
DIN 52612
Melting Point
220
°C
428
°F
DIN 53765
Maximum Service Temperature, Air
100
°C
212
°F
for 50% loss of tensile strength after 20000hr
200
°C
392
°F
Decomposition Temperature
>=
300
°C
>=
572
°F
Ignition Temperature
>=
400
°C
>=
752
°F
ASTM D129
Processing Properties
Metric
English
Comments
Processing Temperature
80.0
°C
176
°F
Hopper Throat
Zone 1
260
°C
500
°F
Feed Zone
Zone 2
270
°C
518
°F
Compression
Zone 3
280
°C
536
°F
Metering-zone
Zone 4
280
°C
536
°F
Nozzle
Melt Temperature
270
-
290
°C
518
-
554
°F
Injection-molding/Extrusion
280
°C
536
°F
Optimal
Mold Temperature
80.0
°C
176
°F
Optimal
80.0
-
90.0
°C
176
-
194
°F
Injection-molding
Drying Temperature
80.0
°C
176
°F
Dry Time
4
hour
4
hour
Moisture Content
0.030 - 0.060 %
0.030 - 0.060 %
Optimal
<= 0.15 %
<= 0.15 %
Descriptive Properties
Color
BK 00564
Commercial Status
Europe
Peripheral Screw Speed
< 0.3 m/s
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
BASF Ultramid® B3GK24 10/20% Glass Bead/Fiber Filled PA6 (Conditioned)
BASF Ultramid® B3GK24 BK 00564 10/20% Glass/Glass Bead Filled PA6 (Dry)
BASF Ultramid® B3GK24 10/20% Glass Bead/Fiber Filled PA6 (Dry)
BASF Basotect UL Foam
BASF Ultradur® B 4040 G10 BK5110 50% Glass Filled PBT
PBASG0281 / 131914
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.