MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

NYCOA NY-FLEX® CT 180 Nylon-Based TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE; Nylon (Polyamide PA)

Material Notes: NY-FLEX® E-TPE grades deliver excellent flexibility at low temperature, superior retention of properties to elevated temperature, exceptional impact toughness and resilience. These also exhibit high creep resistance, strong resistance to flex fatigue, good abrasion resistance, and good resistance to greases, oils, and solvents.

These materials are block copolymers of nylon (polyamide) segments and polyether segments. Physical properties vary with the ratio of the two components.

'Dry' samples tested as-molded - <0.3% moisture. 'Conditioned' samples are equilibrated at 50% RH and 23°C.

Information provided by Nylon Corporation of America.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.11 g/cc0.0401 lb/in³ASTM D792
Water Absorption 3.3 %
@Time 86400 sec
3.3 %
@Time 24.0 hour
ASTM D570
Moisture Absorption at Equilibrium 2.7 %2.7 %50% RH; ASTM D570
Linear Mold Shrinkage 0.011 - 0.013 cm/cm0.011 - 0.013 in/inNYCOA Test
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  73
@Time 15.0 sec
73
@Time 0.00417 hour
Conditioned; ASTM D2240
 76
@Time 0.000 sec
76
@Time 0.000 hour
Conditioned; ASTM D2240
 78
@Time 15.0 sec
78
@Time 0.00417 hour
Dry; ASTM D2240
 80
@Time 0.000 sec
80
@Time 0.000 hour
Dry; ASTM D2240
Tensile Strength 46.0 MPa6670 psiConditioned; ASTM D638
 56.0 MPa8120 psiDry; ASTM D638
Tensile Stress at Strain  23.0 MPa
@Strain 5.0 %
3340 psi
@Strain 5.0 %
Conditioned; ASTM D638
 30.0 MPa
@Strain 10 %
4350 psi
@Strain 10 %
Conditioned; ASTM D638
 32.0 MPa
@Strain 50 %
4640 psi
@Strain 50 %
Conditioned; ASTM D638
 41.0 MPa
@Strain 50 %
5950 psi
@Strain 50 %
Dry; ASTM D638
 43.0 MPa
@Strain 5.0 %
6240 psi
@Strain 5.0 %
Dry; ASTM D638
 45.0 MPa
@Strain 10 %
6530 psi
@Strain 10 %
Dry; ASTM D638
Elongation at Break >= 200 %>= 200 %Dry; ASTM D638
 >= 200 %>= 200 %Conditioned; ASTM D638
Tensile Modulus 0.725 GPa105 ksiConditioned; ASTM D638
 1.52 GPa220 ksiDry; ASTM D638
Flexural Strength 26.0 MPa3770 psiConditioned; ASTM D790
 50.0 MPa7250 psiDry; ASTM D790
Flexural Modulus 0.620 GPa89.9 ksiConditioned; ASTM D790
 1.62 GPa235 ksiDry; ASTM D790
Izod Impact, Notched  0.690 J/cm
@Temperature -30.0 °C
1.29 ft-lb/in
@Temperature -22.0 °F
Dry; ASTM D256
 0.780 J/cm
@Temperature -30.0 °C
1.46 ft-lb/in
@Temperature -22.0 °F
Conditioned; ASTM D256
 1.55 J/cm
@Temperature 23.0 °C
2.90 ft-lb/in
@Temperature 73.4 °F
Dry; ASTM D256
 2.56 J/cm
@Temperature 23.0 °C
4.80 ft-lb/in
@Temperature 73.4 °F
Conditioned; ASTM D256
Izod Impact, Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ASTM D256
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ASTM D256
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Dry; ASTM D256
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Conditioned; ASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 214 °C417 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NYCOA NY-FLEX® CT 145 Nylon-Based TPE
NYCOA NY-FLEX® CT 176 Nylon-Based TPE
NYCOA NY-FLEX® CT 172 Nylon-Based TPE
NYCOA NY-FLEX® CT 164 Nylon-Based TPE
NYCOA NY-FLEX® CT 155 Nylon-Based TPE

PNYCOA90 / 217538

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.