MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Röhm ACRYLITE® LED LD24 Acrylic Polymer  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA)

Material Notes: ACRYLITE® acrylic molding and extrusion compounds have extreme clarity and long-term weatherability. These characteristics are enhanced with the addition of light handling and diffusion properties that can make lighting designs unique and easy to manufacture. ACRYLITE® LED and ACRYLITE® Satinice are used for interior ambient and exterior accent lighting for both general lighting and automotive applications. The LED light molded designs or profile extrusions allow designers to empower the occupant or owner to choose their own lighting color simply by selecting the desired LED color.

Information Provided by Evonik CYRO. The former Evonik Methacrylates business has been sold to Röhm (Roehm) GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³ASTM D729
Water Absorption 0.30 %0.30 %ASTM D570
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inASTM D955
Melt Flow 3.1 g/10 min
@Load 3.80 kg,
Temperature 230 °C
3.1 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 101101ASTM D785
Tensile Strength at Break 80.0 MPa11600 psiASTM D638
Elongation at Break 4.0 - 6.0 %4.0 - 6.0 %ASTM D638
Elongation at Yield 4.0 - 6.0 %4.0 - 6.0 %ASTM D638
Tensile Modulus 3.20 GPa464 ksiASTM D638
Flexural Strength 128.9 MPa18700 psiASTM D790
Flexural Modulus 2.90 GPa421 ksiASTM D790
Izod Impact, Notched (ISO) 0.330 kJ/m²0.157 ft-lb/in²ASTM D256
 
Thermal PropertiesMetricEnglishComments
CTE, linear 130 µm/m-°C
@Temperature 0.000 - 100 °C
72.0 µin/in-°F
@Temperature 32.0 - 212 °F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °C198 °FASTM D648
Vicat Softening Point 108 °C226 °FASTM D1525
Flammability, UL94 HBHB
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.491.49ASTM D542
Haze <= 4.0 %<= 4.0 %ASTM D1003
Yellow Index <= 1.0 %<= 1.0 %ASTM D1925
Transmission, Visible 91 %91 %ASTM D1003

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Röhm Acrylite Plus® zdf Impact Acrylic Polymer
Röhm Acrylite Plus® zk3HR Impact Acrylic Polymer
Röhm Acrylite Plus® zk4BR Impact Acrylic Polymer
Röhm Acrylite Plus® zk4HR Impact Acrylic Polymer
Röhm Acrylite Plus® zk5BR Impact Acrylic Polymer

PEVONIL062 / 196266

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.