MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex Medalist® MD-23143 Thermoplastic Vulcanizate Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Medalist MD-23143 is a high performance thermoplastic vulcanizate specifically designed for healthcare and medical applications. Medalist MD-23143 is a low hardness, low density, sterilizable grade suitable for injection molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Autoclave Sterilizable; Chemical Resistant; Ethylene Oxide Sterilizable; Good Adhesion; Good Processability; Good Sterilizability; Halogen Free; Low Compression Set; Low Density; Low Hardness; Low Specific Gravity; Radiation Sterilizable

Uses: Dental Applications; Gaskets; Hospital Goods; Medical Devices; Medical/Healthcare Applications; Pharmaceuticals; Rubber Replacement

Agency Ratings: ISO 10993 Part 5; ISO 13485

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.910 g/cc0.0329 lb/in³ASTM D792
Melt Flow 25 g/10 min
@Load 5.00 kg,
Temperature 200 °C
25 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  43
@Time 5.00 sec
43
@Time 0.00139 hour
Injection Molded; ASTM D2240
 45
@Time 1.00 sec
45
@Time 0.000278 hour
Injection Molded; ASTM D2240
Tensile Strength at Break 3.63 MPa526 psiDie C, 20 in/min; ASTM D412
Tensile Stress at Strain  1.57 MPa
@Strain 100 %
227 psi
@Strain 100 %
Die C, 20 in/min; ASTM D412
 3.17 MPa
@Strain 300 %
460 psi
@Strain 300 %
Die C, 20 in/min; ASTM D412
Elongation at Break 350 %350 %Die C, 20 in/min; ASTM D412
Tear Strength 18.8 kN/m107 pliDie C, 20 in/min; ASTM D624
Compression Set  18 %
@Temperature 22.8 °C,
Time 79200 sec
18 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ASTM D395B
 31 %
@Temperature 70.0 °C,
Time 79200 sec
31 %
@Temperature 158 °F,
Time 22.0 hour
Type 1; ASTM D395B
 40 %
@Temperature 100 °C,
Time 79200 sec
40 %
@Temperature 212 °F,
Time 22.0 hour
Type 1; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 149 - 171 °C300 - 340 °F
Middle Barrel Temperature 171 - 193 °C340 - 380 °F
Front Barrel Temperature 193 - 216 °C380 - 420 °F
Nozzle Temperature 193 - 216 °C380 - 420 °F
Melt Temperature 193 - 216 °C380 - 420 °F
Mold Temperature 21.1 - 37.8 °C70.0 - 100 °F
Back Pressure 0.172 - 0.689 MPa25.0 - 100 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceColors Available
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-215 Thermoplastic Elastomer
Teknor Apex Uniprene® UN-7010-45NT Thermoplastic Vulcanizate
Teknor Apex Uniprene® UN-7010-40D-NT Thermoplastic Vulcanizate
Teknor Apex Medalist® MD-23153 Thermoplastic Vulcanizate Elastomer
Teknor Apex Medalist® MD-23133 XRD Thermoplastic Vulcanizate Elastomer

PTEKNQ0716 / 237207

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.