MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman Diamond Centrex® 814 General Purpose Injection Molding Grade  (discontinued **)
Categories: Polymer; Thermoplastic; ASA Polymer

Material Notes: Centrex 814 resin is a high-gloss, high-impact grade of ASA (acrylonitrile-styrene-acrylate). It is an injection molding grade with a good balance of physical properties, gloss and processing performance, along with good resistance to weather aging.

Applications: Typical applications for Centrex 814 resin includes exterior parts such as marine components, pool accessories, spa components, lawn and garden accessories, large, outdoor TV screen displays; pool accessories, recreation vehicle components and outdoor advertising sign parts. As with any product, use of Centrex 814 resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

A. Schulman has acquired Network Polymers & Diamond Polymers.

Key Words: Weatherable Polymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0060 cm/cm0.0050 - 0.0060 in/inASTM D955
Melt Flow 9.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
9.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 101101ASTM D785
Tensile Strength, Yield 38.5 MPa5580 psichs 2.0 in/min; ASTM D638
Tensile Modulus 2.10 GPa305 ksichs 2.0 in/min; ASTM D638
Flexural Strength 68.7 MPa9960 psichs 0.05 in/min; ASTM D790
Flexural Modulus 2.20 GPa319 ksitangent; chs 0.05 in/min; ASTM D790
Izod Impact, Notched  0.750 J/cm
@Thickness 3.17 mm,
Temperature -30.0 °C
1.41 ft-lb/in
@Thickness 0.125 in,
Temperature -22.0 °F
ASTM D256
 2.70 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
5.06 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
ASTM D256
Impact Test  8.20 J
@Temperature -30.0 °C
6.05 ft-lb
@Temperature -22.0 °F
ASTM D3763
 33.0 J
@Temperature 23.0 °C
24.3 ft-lb
@Temperature 73.4 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 71.0 °C160 °F0.125";; ASTM D648
 77.0 °C171 °F0.25";; ASTM D648
Vicat Softening Point 101 °C
@Load 1.00 kg
214 °F
@Load 2.20 lb
120°C/hr; ASTM D1525
Flammability, UL94 HB
@Thickness 0.749 mm
HB
@Thickness 0.0295 in

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
INEOS Styrolution Lustran® 256/Lustran® 752 Blended ABS Resin
A. Schulman Diamond ASA S210B
A. Schulman Diamond ASA TW18B3 ASA Weatherable Polymers Injection Molding Grade, Very High Heat
A. Schulman Diamond Centrex® 810 Injection Molding Grade
A. Schulman Diamond Centrex® 821 ASA Weatherable Polymers Injection Molding Grade

PDIAM354 / 126445

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.