MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Supreme Petrochem SP 6450 High Heat Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Heat Resistant Grade

Material Notes: Characteristics
  • High impact and modulus
  • Very good flow properties
  • High heat resistance & strength
  • Available in any dark color
Processing
  • Injection molding
Applications
  • Instrument enclosures
  • Automobile interior parts
  • Telecommunication components
  • HVAC components
Material Status: Commercial : Active

Agency Ratings:

Information provided by Supreme Petrochem LTD

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.04 g/cc1.04 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/inASTM D792
Melt Flow 10 g/10 min
@Load 10.0 kg,
Temperature 200 °C
10 g/10 min
@Load 22.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 36.8 MPa5340 psi50 mm/min; ASTM D638
Elongation at Break 50 %50 %50 mm/min; ASTM D638
Flexural Strength 58.8 MPa
@Thickness 3.20 mm
8530 psi
@Thickness 0.126 in
ASTM D790
Flexural Modulus 1.96 GPa
@Thickness 3.20 mm
284 ksi
@Thickness 0.126 in
ASTM D790
Izod Impact, Notched 1.30 J/cm
@Thickness 3.20 mm
2.44 ft-lb/in
@Thickness 0.126 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmIEC 93
Surface Resistance >= 1.00e+14 ohm>= 1.00e+14 ohmIEC 93
Dielectric Constant 2.6
@Frequency 1e+6 Hz
2.6
@Frequency 1e+6 Hz
IEC 250
Dissipation Factor 0.00040
@Frequency 1e+6 Hz
0.00040
@Frequency 1e+6 Hz
IEC 250
 
Thermal PropertiesMetricEnglishComments
Hot Ball Pressure Test 90.0 °C194 °FIEC335-1
Deflection Temperature at 1.8 MPa (264 psi) 105 °C221 °FASTM D648
Vicat Softening Point 110 °C230 °F5kg / 120°C; ASTM D1525
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 - 280 °C464 - 536 °F
Mold Temperature 40.0 - 80.0 °C104 - 176 °F
Drying Temperature 80.0 °C176 °F( 2 hrs) Pre drying temp.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Supreme Petrochem SP 6460 High Heat Polystyrene
Supreme Petrochem SP 6456 High Heat Polystyrene
Supreme Petrochem SP 556 Flame Retardant Polystyrene
INEOS Styrolution Styrolux® 3G55 SBC
INEOS Styrolution PS 158 N/L GPPS

PSUP22 / 69454

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.