MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AK Steel 410S Ferritic Stainless steel
Categories: Metal; Ferrous Metal; Ferritic; Stainless Steel; T 400 Series Stainless Steel

Material Notes: AK Steel 410S Stainless Steel is a non-hardening modification of Type 410. A small titanium addition minimizes austenite formation at high temperatures, thereby restricting the alloy's ability to harden. The result is a soft, ductile condition when the material is rapidly cooled from above the critical temperature. This non-hardening characteristic also retards formation of hardening cracks when the steel is welded. The alloy is completely ferritic in the annealed condition. AK Steel 410S is particularly useful for annealing boxes, quenching racks, oxidation-resistant partitions and other high temperature units. AK Steel 410S is Ferro-magnetic.

Information provided by AK Steel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.73 g/cc0.279 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 7575Annealed
Tensile Strength, Ultimate 448 MPa65000 psiAnnealed
Tensile Strength, Yield 276 MPa
@Strain 0.2 %
40000 psi
@Strain 0.2 %
Annealed
Elongation at Break 25 %25 %in 2 inches, Annealed
Modulus of Elasticity 200 GPa29000 ksi
Izod Impact 42.0 J31.0 ft-lbV-Notch (Annealed)
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000600 ohm-cm0.0000600 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.8 µm/m-°C
@Temperature 0.000 - 100 °C
6.00 µin/in-°F
@Temperature 32.0 - 212 °F
 13.5 µm/m-°C
@Temperature <=649 °C
7.50 µin/in-°F
@Temperature <=1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 26.9 W/m-K
@Temperature 100 °C
187 BTU-in/hr-ft²-°F
@Temperature 212 °F
Melting Point 1482 - 1532 °C2700 - 2790 °F
Solidus 1482 °C2700 °F
Liquidus 1532 °C2790 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 11.5 - 14.5 %11.5 - 14.5 %
Iron, Fe >= 83.15 %>= 83.15 %As Remainder
Manganese, Mn <= 1.0 %<= 1.0 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti <= 0.20 %<= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AK Steel 304 Austenitic Stainless steel
AK Steel 301 Austenitic Stainless steel
AK Steel 439 Ferritic Stainless steel
405 Stainless Steel, annealed, sheet
AK Steel 430 Ferritic Stainless steel

NAKS095 / 14698

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.