MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 6, Glass Filled, Impact Grade
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Glass Filled, Impact Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Glass Filled, Impact Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.15 - 1.53 g/cc0.0415 - 0.0553 lb/in³Average value: 1.29 g/cc Grade Count:148
 1.16 - 1.16 g/cc
@Temperature >=220 °C
0.0419 - 0.0419 lb/in³
@Temperature >=428 °F
Average value: 1.16 g/cc Grade Count:1
Filler Content 5.00 - 50.0 %5.00 - 50.0 %Average value: 28.2 % Grade Count:11
Water Absorption 0.600 - 7.00 %0.600 - 7.00 %Average value: 1.78 % Grade Count:80
Moisture Absorption at Equilibrium 1.40 - 2.50 %1.40 - 2.50 %Average value: 1.90 % Grade Count:45
Water Absorption at Saturation 4.80 - 8.50 %4.80 - 8.50 %Average value: 6.46 % Grade Count:30
Viscosity Test 150 cm³/g1.50 dl/gAverage value: 150 cm³/g Grade Count:3
Linear Mold Shrinkage 0.000900 - 0.0120 cm/cm0.000900 - 0.0120 in/inAverage value: 0.00451 cm/cm Grade Count:94
Linear Mold Shrinkage, Transverse 0.00100 - 0.0140 cm/cm0.00100 - 0.0140 in/inAverage value: 0.00682 cm/cm Grade Count:43
Melt Flow 1.00 - 45.0 g/10 min1.00 - 45.0 g/10 minAverage value: 18.9 g/10 min Grade Count:7
Ash 30.0 - 36.0 %30.0 - 36.0 %Average value: 32.3 % Grade Count:4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 76.0 - 12176.0 - 121Average value: 83.9 Grade Count:13
Hardness, Rockwell R 82.0 - 12082.0 - 120Average value: 114 Grade Count:25
Ball Indentation Hardness 80.0 - 220 MPa11600 - 31900 psiAverage value: 149 MPa Grade Count:7
Tensile Strength, Ultimate 40.0 - 200 MPa5800 - 29000 psiAverage value: 111 MPa Grade Count:140
Tensile Strength, Yield 6.00 - 170 MPa870 - 24700 psiAverage value: 103 MPa Grade Count:12
Elongation at Break 2.20 - 28.0 %2.20 - 28.0 %Average value: 5.35 % Grade Count:142
Elongation at Yield 2.90 - 8.00 %2.90 - 8.00 %Average value: 4.96 % Grade Count:6
Modulus of Elasticity 1.70 - 13.8 GPa247 - 2000 ksiAverage value: 6.54 GPa Grade Count:76
Flexural Yield Strength 55.0 - 290 MPa7980 - 42100 psiAverage value: 164 MPa Grade Count:105
Flexural Modulus 2.10 - 11.7 GPa305 - 1700 ksiAverage value: 5.71 GPa Grade Count:108
Compressive Yield Strength 62.1 - 172 MPa9000 - 24900 psiAverage value: 119 MPa Grade Count:14
Poissons Ratio 0.3500.350Average value: 0.350 Grade Count:11
Shear Modulus 1.60 - 4.40 GPa232 - 638 ksiAverage value: 3.15 GPa Grade Count:8
Izod Impact, Notched 0.640 - 2.75 J/cm1.20 - 5.14 ft-lb/inAverage value: 1.63 J/cm Grade Count:37
Izod Impact, Unnotched 5.82 J/cm - NB10.9 ft-lb/in - NBAverage value: 10.1 J/cm Grade Count:12
Izod Impact, Notched (ISO) 10.0 - 40.0 kJ/m²4.76 - 19.0 ft-lb/in²Average value: 18.8 kJ/m² Grade Count:45
 8.00 - 20.0 kJ/m²
@Temperature -40.0 - -30.0 °C
3.81 - 9.52 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 13.1 kJ/m² Grade Count:13
Izod Impact, Unnotched (ISO) 55.0 - 90.0 kJ/m²26.2 - 42.8 ft-lb/in²Average value: 73.0 kJ/m² Grade Count:6
 40.0 - 79.0 kJ/m²
@Temperature -30.0 - -30.0 °C
19.0 - 37.6 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 61.1 kJ/m² Grade Count:6
Charpy Impact Unnotched 5.00 J/cm² - NB23.8 ft-lb/in² - NBAverage value: 8.80 J/cm² Grade Count:52
 4.50 - 11.5 J/cm²
@Temperature -40.0 - -20.0 °C
21.4 - 54.7 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 7.61 J/cm² Grade Count:32
Charpy Impact, Notched 0.700 - 4.20 J/cm²3.33 - 20.0 ft-lb/in²Average value: 2.00 J/cm² Grade Count:89
 0.610 - 2.52 J/cm²
@Temperature -30.0 - -20.0 °C
2.90 - 12.0 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 1.29 J/cm² Grade Count:29
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+12 - 1.00e+15 ohm-cm1.00e+12 - 1.00e+15 ohm-cmAverage value: 4.19e+14 ohm-cm Grade Count:56
Surface Resistance 1.00e+10 - 1.00e+16 ohm1.00e+10 - 1.00e+16 ohmAverage value: 8.98e+14 ohm Grade Count:34
Dielectric Constant 3.30 - 14.03.30 - 14.0Average value: 5.67 Grade Count:27
Dielectric Strength 19.7 - 40.0 kV/mm500 - 1020 kV/inAverage value: 31.8 kV/mm Grade Count:34
Dissipation Factor 0.00900 - 0.3000.00900 - 0.300Average value: 0.105 Grade Count:15
Dielectric Loss Index 0.0200 - 0.2200.0200 - 0.220Average value: 0.113 Grade Count:12
Arc Resistance 120 - 180 sec120 - 180 secAverage value: 160 sec Grade Count:3
Comparative Tracking Index 450 - 600 V450 - 600 VAverage value: 543 V Grade Count:22
 
Thermal PropertiesMetricEnglishComments
CTE, linear 3.00 - 50.4 µm/m-°C1.67 - 28.0 µin/in-°FAverage value: 27.4 µm/m-°C Grade Count:32
 27.0 - 27.0 µm/m-°C
@Temperature 35.0 - 55.0 °C
15.0 - 15.0 µin/in-°F
@Temperature 95.0 - 131 °F
Average value: 27.0 µm/m-°C Grade Count:1
 27.0 - 27.0 µm/m-°C
@Thickness 2.00 - 2.00 mm
15.0 - 15.0 µin/in-°F
@Thickness 0.0787 - 0.0787 in
Average value: 27.0 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 59.4 - 130 µm/m-°C33.0 - 72.2 µin/in-°FAverage value: 95.6 µm/m-°C Grade Count:19
Thermal Conductivity 0.200 - 0.389 W/m-K1.39 - 2.70 BTU-in/hr-ft²-°FAverage value: 0.312 W/m-K Grade Count:3
Melting Point 205 - 225 °C401 - 437 °FAverage value: 218 °C Grade Count:84
Maximum Service Temperature, Air 90.0 - 180 °C194 - 356 °FAverage value: 135 °C Grade Count:9
Deflection Temperature at 0.46 MPa (66 psi) 193 - 220 °C380 - 428 °FAverage value: 209 °C Grade Count:62
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 495 °C158 - 923 °FAverage value: 197 °C Grade Count:99
Deflection Temperature at 8.0 MPa 55.0 - 120 °C131 - 248 °FAverage value: 94.0 °C Grade Count:5
Vicat Softening Point 185 - 215 °C365 - 419 °FAverage value: 199 °C Grade Count:19
Minimum Service Temperature, Air -60.0 °C-76.0 °FAverage value: -60.0 °C Grade Count:3
Flammability, UL94 HBHBGrade Count:63
Glow Wire Test 550 - 650 °C1020 - 1200 °FAverage value: 617 °C Grade Count:9
 
Processing PropertiesMetricEnglishComments
Processing Temperature 221 - 290 °C430 - 554 °FAverage value: 264 °C Grade Count:21
Nozzle Temperature 210 - 288 °C410 - 550 °FAverage value: 250 °C Grade Count:3
Melt Temperature 220 - 300 °C428 - 572 °FAverage value: 261 °C Grade Count:54
Mold Temperature 43.0 - 121 °C109 - 250 °FAverage value: 82.5 °C Grade Count:66
Injection Velocity 30.0 - 60.0 mm/sec1.18 - 2.36 in/secAverage value: 45.0 mm/sec Grade Count:3
Drying Temperature 75.0 - 100 °C167 - 212 °FAverage value: 83.7 °C Grade Count:43
Moisture Content 0.0300 - 0.200 %0.0300 - 0.200 %Average value: 0.154 % Grade Count:27
Injection Pressure 30.0 - 130 MPa4350 - 18900 psiAverage value: 83.3 MPa Grade Count:15

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Glass Bead Filled
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Overview of materials for Nylon 6, 10% Glass Fiber Filled
Overview of materials for Nylon 6, Impact Grade
Overview of materials for Nylon 6, MoS2 Filled

O2417 / 77977

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.