MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Ultramid® S3WG6 Balance 30% Glass Filled PA 610 (Conditioned)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 610 (PA610); Nylon 610, Glass Reinforced

Material Notes: Description: BASF supplies polyamide 610 for processing by injection molding under the trade name Ultramid® Balance which is produced by polycondensation of hexamethylene diamine and sebacic acid. This means that more than 60 % of the base polymer for the product family consists of sustainable raw materials. Ultramid® S Balance is highly resistant to fuels, oils and greases, to most solvents, aqueous solutions and alkalis. Its resistance to weakly acid media makes it superior to PA 6 and PA 66.
    Applications:
  • Overmolding metal and electronic components that come into contact with aggressive media, for example wheel speed sensors
  • Housing and gear components where dimensional stability is a major consideration
  • plug-in connectors, pipes and reservoirs in cooling circuits with high demands on hydrolysis resistance

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.31 g/cc0.0473 lb/in³ISO 1183
Water Absorption 2.0 - 2.6 %2.0 - 2.6 %ISO 62
Moisture Absorption at Equilibrium 0.80 - 1.2 %0.80 - 1.2 %ISO 62
Viscosity Test 150 cm³/g1.50 dl/gISO 307
Linear Mold Shrinkage 0.0040 cm/cm0.0040 in/inTest Box 1.5 mm
Linear Mold Shrinkage, Flow 0.0040 cm/cm0.0040 in/inISO 2577
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inISO 2577
Melt Flow 39.3 g/10 min
@Load 5.00 kg,
Temperature 275 °C
39.3 g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 110 MPa16000 psiISO 527-1/-2
Elongation at Yield 6.0 %6.0 %ISO 527-1/-2
Modulus of Elasticity 6.20 GPa899 ksiISO 527-1/-2
Flexural Strength 160 MPa23200 psiISO 178
Flexural Modulus 5.60 GPa812 ksiISO 178
Charpy Impact Unnotched 9.00 J/cm²
@Temperature 23.0 °C
42.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FISO 11357-1/-3
 
Processing PropertiesMetricEnglishComments
Melt Temperature 270 - 290 °C518 - 554 °FInjection molding
Mold Temperature 80.0 - 90.0 °C176 - 194 °FInjection molding
 
Descriptive Properties
Commercial StatusEurope

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® S3WG6 Balance 30% Glass Filled PA 610 (Dry)
BASF Ultramid® S3K Balance PA 610 (Dry)
BASF Ultramid® S3K Balance PA 610 (Conditioned)
BASF Ultramid® S3WG7 Balance 35% Glass Filled PA 610 (Dry)
BASF Ultramid® S3WG7 Balance 35% Glass Filled PA 610 (Conditioned)

PBASG0341 / 131974

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.