MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Avient Edgetek® X TR2-20TA/000 NATURAL Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: The Edgetek™ engineering thermoplastics compounds made with Eastman Tritan™ copolyester offer a wide range of performance and properties with the addition of reinforcing additives. By utilizing Eastman Tritan™ copolyester these compounds provide chemical resistance, clarity, heat resistance and BPA-free solutions.

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.33 g/cc1.33 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0020 - 0.0030 cm/cm
@Thickness 3.18 mm
0.0020 - 0.0030 in/in
@Thickness 0.125 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 40.7 MPa5900 psiType I, 5.1 mm/min; ASTM D638
Tensile Strength, Yield 51.7 MPa7500 psi5.1 mm/min; ASTM D638
Elongation at Break 30 %30 %Type I, 5.1 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %5.1 mm/min; ASTM D638
Tensile Modulus 3.38 GPa490 ksiType I, 5.1 mm/min; ASTM D638
Flexural Strength 89.6 MPa13000 psi1.3 mm/min; ASTM D790
Flexural Modulus 3.03 GPa439 ksi1.3 mm/min; ASTM D790
Izod Impact, Notched 0.750 J/cm
@Thickness 3.18 mm,
Temperature 23.0 °C
1.41 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Injection Molded; ASTM D256A
Izod Impact, Unnotched 21.0 J/cm
@Thickness 3.18 mm,
Temperature 23.0 °C
39.3 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
Injection Molded, Partial Break; ASTM D256
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C
@Temperature -30.0 - 30.0 °C
61.1 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM E831
CTE, linear, Transverse to Flow 140 µm/m-°C
@Temperature -30.0 - 30.0 °C
77.8 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 112 °C
@Thickness 3.18 mm
234 °F
@Thickness 0.125 in
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 103 °C
@Thickness 3.18 mm
217 °F
@Thickness 0.125 in
Unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Melt Temperature 266 - 282 °C511 - 540 °F
Mold Temperature 60.0 - 65.6 °C140 - 150 °F
Drying Temperature 87.8 °C190 °F
Dry Time 4.00 hour4.00 hour
 
Descriptive Properties
FeaturesBPA Free
 Crazing Resistant
 Filled
 Good Chemical Resistance
 Good Crack Resistance
 Good Dimensional Stability
 Good Toughness
 Medium Clarity
 Medium Heat Resistance
Filler / ReinforcementMineral Filler
FormsPellets
Generic MaterialCopolyester
Generic NameCopolyester
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
UsesAppliance Components
 Consumer Applications
 Food Service Applications
 Household Goods
 Industrial Applications

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Eastman Tritan™ TX2000 Copolyester
Avient Edgetek® X TR2-10TA/000 NATURAL Copolyester
Eastman Tritan™ TX2001 Copolyester
Celanese Celanex® 2025 Copolyester
Eastman Tritan™ MX810 Medical Grade Copolyester

PH0POL1037 / 145606

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.