ICE Al2O3 99.8
Categories:
Ceramic
;
Oxide
;
Aluminum Oxide
Material Notes:
Data provided by the manufacturer, International Ceramic Engineering.
Key Words:
ICE Al2O3 99.8 aluminas, International Ceramic Engineering; aluminum oxide, aluminium oxide, aluminas
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
3.92
g/cc
0.142
lb/in³
Water Absorption
0.00 %
0.00 %
Mechanical Properties
Metric
English
Comments
Hardness, Mohs
9.0
9.0
Tensile Strength, Ultimate
150
MPa
21800
psi
Flexural Strength
300
MPa
43500
psi
Compressive Strength
2400
MPa
348000
psi
Fracture Toughness
4.50
MPa-m½
4.10
ksi-in½
Electrical Properties
Metric
English
Comments
Dielectric Constant
9.3
@Frequency 1e+6 Hz
9.3
@Frequency 1e+6 Hz
Dielectric Strength
9.10
kV/mm
231
kV/in
Dielectric Loss Index
0.0016
@Frequency 1e+6 Hz
0.0016
@Frequency 1e+6 Hz
Thermal Properties
Metric
English
Comments
CTE, linear
7.40
µm/m-°C
@Temperature 25.0 - 600 °C
4.11
µin/in-°F
@Temperature 77.0 - 1110 °F
Thermal Conductivity
38.9
W/m-K
270
BTU-in/hr-ft²-°F
Maximum Service Temperature, Air
1750
°C
3180
°F
Component Elements Properties
Metric
English
Comments
Al2O3
99.8 %
99.8 %
Descriptive Properties
Color
Ivory
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
ICE Al2O3 99.5
Overview - Alumina, 96%, Al
2
O
3
99.5% Alumina, porous body
AISI 1044 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
Ferro Aluminum Oxide P87
CI0004 / 1380
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.