MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Cossa Polimeri ESTALUX 9202 Methyl Methacrylate Acrylonitrile Butadiene Styrene
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylic (PMMA)

Material Notes: Plastic blend that combines impact properties of ABS with the excellent transparency of PMMA

Biomedical grade in line with US pharmacopeia class VI USP and European pharmacopeia cap. 3.2.2

Information provided by Cossa Polimeri S.r.l.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.07 g/cc0.0387 lb/in³ASTM D 792
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inASTM D 955
Melt Flow  2.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
2.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D 1238
 18 g/10 min
@Load 21.6 kg,
Temperature 220 °C
18 g/10 min
@Load 47.6 lb,
Temperature 428 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 35.0 MPa5080 psiASTM D 638
Tensile Strength, Yield 45.0 MPa6530 psiASTM D 638
Elongation at Break 4.0 %4.0 %ASTM D 638
Tensile Modulus 2.05 GPa297 ksiASTM D 638
Flexural Modulus 1.90 GPa276 ksiASTM D 790
Izod Impact, Notched 0.800 J/cm
@Temperature 23.0 °C
1.50 ft-lb/in
@Temperature 73.4 °F
ASTM D 256
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point  95.0 °C
@Load 5.10 kg
203 °F
@Load 11.2 lb
120°C/hr; ASTM D 1525
 108 °C
@Load 1.02 kg
226 °F
@Load 2.25 lb
120°C/hr; ASTM D 1525
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 220 - 240 °C428 - 464 °F
Mold Temperature 40.0 - 60.0 °C104 - 140 °F
Dry Time 2.00 - 4.00 hour
@Temperature 80.0 °C
2.00 - 4.00 hour
@Temperature 176 °F
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cossa Polimeri ESTALUX 9202 A Methyl Methacrylate Acrylonitrile Butadiene Styrene
Cossa Polimeri ESTALUX 5513 Methyl Methacrylate Acrylonitrile Butadiene Styrene
Cossa Polimeri ESTALUX 9206 A Methyl Methacrylate Acrylonitrile Butadiene Styrene
Cossa Polimeri ESTALUX 9206 Methyl Methacrylate Acrylonitrile Butadiene Styrene
Trinseo Plexiglas® SG7 Acrylic

PCOSSA917 / 156507

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.