MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow 621I Low Density Polyethylene (LDPE)
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes:
  • Specialty resin designed for high melt strength applications
  • Provides excellent bubble stability
  • Complies with U.S. FDA 21 CFR 177.1520 (c) 2.1

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.918 g/cc0.0332 lb/in³ASTM D792
Thickness 50.8 microns2.00 mil
Melt Flow 2.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.3 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 11.64 MPa1688 psiASTM D882
Film Tensile Strength at Yield, TD 11.02 MPa1598 psiASTM D882
Film Elongation at Break, MD 451 %451 %ASTM D882
Film Elongation at Break, TD 620 %620 %ASTM D882
Secant Modulus, MD 0.1662 GPa24.11 ksi2% Secant; ASTM D882
Secant Modulus, TD 0.2081 GPa30.18 ksi2% Secant; ASTM D882
Impact 4343[ft-lbf/in3]; Puncture Resistance; Dow Method
 16951695[ft-lbf/in3]; Toughness MD; ASTM D882
 17901790[ft-lbf/in3]; Toughness TD; ASTM D882
Elmendorf Tear Strength MD 321 g321 gASTM D1922
Elmendorf Tear Strength TD 189 g189 gASTM D1922
Elmendorf Tear Strength, MD 6.319 g/micron160.5 g/milASTM D1922
Elmendorf Tear Strength, TD 3.72 g/micron94.5 g/milASTM D1922
Dart Drop Test 96.0 g0.212 lbMethod A; ASTM D1709
Film Tensile Strength at Break, MD 21.75 MPa3155 psiASTM D882
Film Tensile Strength at Break, TD 19.62 MPa2845 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 108 °C226 °FDow Method (DSC)
Vicat Softening Point 92.0 °C198 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 16.1 %16.1 %ASTM D1003
Gloss 40 %40 %45°; ASTM D2457
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont 20 Series 20-6064 Specialty Polyethylene Resin
Dow 662I Low Density Polyethylene Resin
Dow 650I Low Density Polyethylene Resin
Dow 620I Linear Low Density Polyethylene (LDPE)
Dow 611A Low Density Polyethylene (LDPE)

PDOW1489 / 30707

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.