MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Celanese Crastin® SK601 BK851 PBT-GF10
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

Material Notes: 10% Glass Reinforced Polybutylene Terephthalate

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.37 g/cc0.0495 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0070 cm/cm0.0070 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 80.0 MPa11600 psiISO 527-1/-2
Elongation at Break 4.2 %4.2 %ISO 527-1/-2
Tensile Modulus 4.40 GPa638 ksiISO 527-1/-2
Flexural Strength 140 MPa20300 psiISO 178
Poissons Ratio 0.360.36
Izod Impact, Notched (ISO) 4.00 kJ/m²
@Temperature 23.0 °C
1.90 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched  3.50 J/cm²
@Temperature -30.0 °C
16.7 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 250 V250 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 225 °C437 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 180 °C356 °FISO 75-1/-2
Glass Transition Temp, Tg 55.0 °C131 °F10°C/min; ISO 11357-1/-2
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
IEC 60695-11-10
Flame Spread 36.0 mm/min
@Thickness 1.00 mm
1.42 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 20 %20 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 °C482 °FOptimum, Injection
 240 - 260 °C464 - 500 °FRange, Injection
Mold Temperature 80.0 °C176 °FOptimum, Injection
 30.0 - 130 °C86.0 - 266 °FInjection
Ejection Temperature 170 °C338 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.040 %<= 0.040 %Injection
Hold Pressure >= 60.0 MPa>= 8700 psiInjection
 
Descriptive Properties
Back pressureAs low as possible
Drying RecommendedyesInjection
Emission of organic compounds (µgC/g)72VDA 277
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging (mg)0.1G-value (condensate); ISO 6452
Odor Class3VDA 270
Part Marking Code>PBT-GF10<ISO 11469
PolymerPBT-GF10
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPBT-GF10ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Crastin® SK603 BK851 PBT-GF20
Envalior Arnite® TV6 220 PBT-GF10
Celanese Crastin® SK605 BK851 PBT-GF30
Envalior Pocan® B 4225 000000 PBT, 20% Glass Fiber
Envalior Pocan® B 3235 901510 PBT, 30% Glass Fiber

PDSX5051 / 197691

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.