MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Fire-refined Tough Pitch Copper with Silver, UNS C12800, H08 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability; good forgeability. Fabricated by coining, coppersmithing, drawing and upsetting, hot forging and pressing, spinning, swaging, stamping.

Applications: busbars, bus conductors, waveguides, hollow conductors, lead-in wires and anodes for vacuum tubes, vacuum seals, transistor components, glass to metal seals, coaxial cables and tubes, klystrons, microwave tubes, and rectifiers.

Test specimens: flat products - 1mm thickness.

UNS C12800 is inactive per the Copper Development Association. C12500, C12700, C12800, C12900, and C13000 are similar alloys having very similar mechanical properties; they are distinguished by differences in silver content.

Key Words: Fire-Refined Copper, FRTSP. MIL-W-3318
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.89 g/cc0.321 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 6060
Hardness, Rockwell F 9494
Hardness, Rockwell 30T 6363
Tensile Strength, Ultimate 380 MPa55100 psi
Tensile Strength, Yield  345 MPa
@Strain 0.5 %
50000 psi
@Strain 0.5 %
 360 MPa
@Strain 0.2 %
52200 psi
@Strain 0.2 %
Elongation at Break 4.0 %4.0 %In 50 mm
Modulus of Elasticity 115 GPa16700 ksiEstimated from similar Cu Alloys
Poissons Ratio 0.310.31Calculated
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 44.0 GPa6380 ksiEstimated from similar Cu Alloys
Shear Strength 200 MPa29000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000176 ohm-cm
@Temperature 20.0 °C
0.00000176 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.8 µm/m-°C
@Temperature 20.0 - 100 °C
9.33 µin/in-°F
@Temperature 68.0 - 212 °F
 17.4 µm/m-°C
@Temperature 20.0 - 200 °C
9.67 µin/in-°F
@Temperature 68.0 - 392 °F
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
9.83 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.385 J/g-°C0.0920 BTU/lb-°F
Thermal Conductivity 377 W/m-K
@Temperature 20.0 °C
2620 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point <= 1085 °C<= 1985 °F
Liquidus 1085 °C1985 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 400 - 650 °C752 - 1200 °F
Hot-Working Temperature 750 - 950 °C1380 - 1740 °F
 
Component Elements PropertiesMetricEnglishComments
Antimony, Sb <= 0.0030 %<= 0.0030 %
Arsenic, As <= 0.012 %<= 0.012 %
Bismuth, Bi <= 0.0030 %<= 0.0030 %
Copper, Cu >= 99.88 %>= 99.88 %Includes Ag
Lead, Pb <= 0.0040 %<= 0.0040 %
Nickel, Ni <= 0.050 %<= 0.050 %
Selenium, Se <= 0.025 %<= 0.025 %includes Te
Silver, Ag >= 0.034 %>= 0.034 %Min 10 troy oz./ton (may be specified)

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zirconium Copper (Amzirc Brand Copper), UNS C15000, 13 mm rod
ZHC Copper, UNS C15100, H08 Temper
Sulfur bearing Copper, UNS C14700, H04 Temper 6 mm rod
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H08 Temper wire
Copper, UNS C15710, 0.8 mm wire, 99.8% Cold Worked

MC12800b6 / 148813

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.