MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ineos R01C-00 Polypropylene Random Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Grade R01C-00 is a low flow rate, high clarity random copolymer designed for extrusion, thermoforming and blow molding, through it is clarifier/antistat additive combination. Applications that require good see-through clarity combined with good heat resistance and refrigerator temperature impact properties can benefit from the use of grade R01C-00. This material meets the requirements of the U.S. Food and Drug Administration as specified in 21 CFR 177.1520.

Applications

  • Thermoformed packaging (cups, containers, lidding)
  • Extrusion blow molded containers and bottles
  • Injection blow molded containers and bottles
  • Extruded sheet and profiles
Benefits
  • Excellent clarity
  • Excellent processability
  • Good impact resistance at room and refrigerator temperatures
  • Low static charge

Key Words: High clarity random copolymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.904 g/cc0.0327 lb/in³ASTM D792
Melt Flow 1.9 g/10 min
@Load 2.16 kg,
Temperature 230 °C
1.9 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 7979ASTM D785
Tensile Strength at Break 19.0 MPa2760 psi2.0 in/min; ASTM D638
Tensile Strength, Yield 28.2 MPa4090 psi2.0 in/min; ASTM D638
Elongation at Break 350 %350 %2.0 in/min; ASTM D638
Elongation at Yield 14 %14 %2.0 in/min; ASTM D638
Flexural Modulus, 1% Secant 1080 MPa156000 psiASTM D790A
Izod Impact, Notched  0.427 J/cm
@Temperature 3.89 °C
0.800 ft-lb/in
@Temperature 39.0 °F
ASTM D256
 2.99 J/cm
@Temperature 22.8 °C
5.60 ft-lb/in
@Temperature 73.0 °F
ASTM D256
Izod Impact, Notched (ISO)  4.30 kJ/m²
@Temperature 3.89 °C
2.05 ft-lb/in²
@Temperature 39.0 °F
Area; ASTM D256
 29.2 kJ/m²
@Temperature 22.8 °C
13.9 ft-lb/in²
@Temperature 73.0 °F
Area; ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 80.0 °C176 °FUnannealed; ASTM D648
Vicat Softening Point 133 °C271 °FASTM D1525
UL RTI, Electrical 65.0 °C
@Thickness 1.52 mm
149 °F
@Thickness 0.0600 in
UL 746
UL RTI, Mechanical with Impact 65.0 °C
@Thickness 1.52 mm
149 °F
@Thickness 0.0600 in
UL 746
UL RTI, Mechanical without Impact 65.0 °C
@Thickness 1.52 mm
149 °F
@Thickness 0.0600 in
UL 746
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
 
Optical PropertiesMetricEnglishComments
Haze 12 %
@Thickness 1.27 mm
12 %
@Thickness 0.0500 in
ASTM D1003
Gloss 100 %100 %60°; ASTM D2457
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.
 
Descriptive Properties
processBlow Molding
 Extrusion
 Injection Molding
 Thermoforming

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Flint Hills 23H2A Random Copolymer Polypropylene
Ineos R12C-00 Polypropylene Random Copolymer
Ineos R12C-01 Polypropylene Random Copolymer
Ineos R01C-01 Polypropylene Random Copolymer
Ineos R01A-00 Polypropylene Random Copolymer

PINEOS009 / 48177

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.