MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Master Bond EP46HT-1AO Two Component Epoxy
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive; Epoxy, High Temperature

Material Notes: Key Features:
  • Impressive thermal conductivity
  • Splendid electrical insulation values
  • High glass transition temperature
  • Very long open times at room temperature
  • Wide temperature range of -100°F to +550°F
  • High quality bonding strength
Product Description: Master Bond EP46HT-1AO is a two component high performance epoxy offering high caliber thermal conductivity, superior electrical insulation and top shelf temperature resistance. It is primarily used for bonding and sealing. The service temperature range is eye-catching at -100°F to +550°F. While it does not cure at room temperature, it does cure readily at elevated temperatures. A good curing schedule to optimize properties is 2 hours at 300°F, followed by a few hours at 350-400°F. Some other noteworthy and desirable properties include exceptional physical strength properties and sterling dimensional stability. EP46HT-1AO has a forgiving 100 to 30-35 mix ratio by weight. It should be noted that EP46HT-1AO is relatively exothermic and should not be cured in sections greater than 20-30 thousandths of an inch thick and a bondline thickness is typically 2-7 thousandths of an inch. EP46HT-1AO withstands rigorous thermal cycling and has striking chemical resistance to oils, water, acids, bases and solvents. It bonds terrifically well to metals, composites, glass, ceramics and many plastics. Once cured, the system is a top flight electrical insulator. The color of Part A is tan and Part B is moderately dark brown. EP46HT-1AO is normally recommended for challenging applications found in the electronic, aerospace and specialty OEM industries where the blend of highly desirable properties discussed above is needed.

Product Advantages:

  • Easy application: contact pressure only required for cure, system spreads evenly and smoothly
  • Working life over 24 hours at room temperature
  • Convenient cure schedules at elevated temperatures
  • Commendable thermal conductivity along with first rate electrical insulation properties
  • Sound dimensional stability and physical strength properties
  • Robust chemical resistance
  • Impressive thermal stability and heat resistance

Information provided by Master Bond Inc.

Vendors: Master Bond is a leading manufacturer of adhesives, sealants, coatings and potting compounds. Master Bond’s vast product line consists of over 3,000 epoxy, polyurethane, silicone, cyanoacrylate and latex adhesives that vary in viscosity, cure speed, strength, chemical resistance, electrical properties, etc. Our custom adhesives offer design flexibility and provide excellent bonding performance. Visit www.masterbond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Viscosity  20000 - 40000 cP
@Temperature 23.9 °C
20000 - 40000 cP
@Temperature 75.0 °F
Part B, thixotropic
 7500 - 150000 cP
@Temperature 23.9 °C
7500 - 150000 cP
@Temperature 75.0 °F
mixed, thixotropic
 200000 - 400000 cP
@Temperature 50.0 °C
200000 - 400000 cP
@Temperature 122 °F
Part A, thixotropic
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 85 - 9585 - 95
Tensile Strength 48.3 - 55.2 MPa7000 - 8000 psi
Elongation at Break 2.0 - 5.0 %2.0 - 5.0 %
Tensile Modulus 3.79 - 4.48 GPa550 - 650 ksi
Compressive Strength 179 - 193 MPa26000 - 28000 psi
Adhesive Bond Strength 9.65 - 11.0 MPa1400 - 1600 psiTensile lap, Aluminum to Aluminum
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cm
Dielectric Strength 17.7 kV/mm
@Thickness 3.17 mm
450 kV/in
@Thickness 0.125 in
 
Thermal PropertiesMetricEnglishComments
CTE, linear 21.0 - 24.0 µm/m-°C11.7 - 13.3 µin/in-°F
Thermal Conductivity 1.30 - 1.44 W/m-K9.02 - 9.99 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 288 °C550 °F
Minimum Service Temperature, Air -73.3 °C-100 °F
Glass Transition Temp, Tg 215 - 220 °C419 - 428 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 120 min2.00 hourPost cure for optimum properties at 350-400°F
 120 - 180 min
@Temperature 121 - 149 °C
2.00 - 3.00 hour
@Temperature 250 - 300 °F
Working Life >= 1440 min>= 1440 minAfter mixing, 100 g batch
Shelf Life 6.00 Month
@Temperature <=23.9 °C
6.00 Month
@Temperature <=75.0 °F
in original, unopened containers
 
Descriptive Properties
Mixing Ratio100:30-35 by weightParts A to B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Master Bond EP21TDC-2AO Flexibilized, Thermally Conductive Two Component Epoxy
Master Bond EP46HT-2AO Black Thermally Conductive, Electrically Insulating Epoxy
Master Bond EP36AO One Part, Thermally Conductive, Heat Resistant Epoxy
Master Bond EP21TDC-2LOND Two Component Epoxy

PMASTM884 / 185477

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.