MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mitsubishi Xantar® LDS 3734 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LDS is becoming increasingly popular as the MID technology to enable an increased number of novel functions available inside appealing housings and covers, such as smart phones and notebooks. With LDS, tailored plastic materials are activated locally using a laser, and subsequently metalized exclusively in the activated areas, thus enabling a fast, highly flexible, 3D-design of, for instance, antennas in existing parts such as covers and frames. The XANTAR LDS portfolio is ideally suited for integrated mobile phone antennas from antenna carriers to fully integrated antennas in the housing or frame. The application area has now been extended to antennas in laptops and notebooks. Full Color custom-made PC- and PC/ABS-based grades are available that enable selective electroless plating by means of laser direct structuring (LDS) to integrate electric circuits into molded parts. For parts that require soldering, specially developed high-temperature Reny® LDS grades are available. Benefits of XANTAR® LDS for laser direct structuring technology (based on joint development with LPKF): Highest-impact material available for laser direct structuring. Halogen free flame retardant. Resolution (line/space) down to 100 microns. Extremely well suited for antennas in mobile phones and notebooks. Full color availability for PC- and PC/ABS based LDS grades. High-performance/robustness: Dielectric constant of PC/ABS helps to assure high antenna performance. Outstanding impact strength outperforms competitive PC-blends. Advantages of innovative LDS technology: Higher flexibility compared to other molded interconnect device (MID) technologies, providing faster time-to-market. Enables 3D shapes and electrical connections simultaneously. Suitable for relatively small surface areas. Only three process steps: molding, laser processing, metallization.

Information provided by Mitsubishi Engineering Plastics Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.29 g/cc0.0466 lb/in³
Water Absorption 0.35 %0.35 %
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/in
Melt Index of Compound 11 g/10 min
@Load 5.00 kg,
Temperature 260 °C
11 g/10 min
@Load 11.0 lb,
Temperature 500 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 50.0 MPa7250 psi
Elongation at Break >= 50 %>= 50 %
Elongation at Yield 6.0 %6.0 %
Tensile Modulus 2.20 GPa319 ksi
Flexural Strength 78.0 MPa11300 psi
Flexural Modulus 2.00 GPa290 ksi
Izod Impact, Notched (ISO)  35.0 kJ/m²
@Temperature -20.0 °C
16.7 ft-lb/in²
@Temperature -4.00 °F
 50.0 kJ/m²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Charpy Impact, Notched  2.50 J/cm²
@Temperature -30.0 °C
11.9 ft-lb/in²
@Temperature -22.0 °F
 4.50 J/cm²
@Temperature 23.0 °C
21.4 ft-lb/in²
@Temperature 73.4 °F
Puncture Energy 40.0 J29.5 ft-lb
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cm
Surface Resistance 1.00e+15 ohm1.00e+15 ohm
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 60.0 µm/m-°C33.3 µin/in-°F
CTE, linear, Transverse to Flow 60.0 µm/m-°C33.3 µin/in-°F
Deflection Temperature at 1.8 MPa (264 psi) 120 °C248 °F
Vicat Softening Point 142 °C
@Load 5.10 kg
288 °F
@Load 11.2 lb
rate 50°C/h
Flammability, UL94 HB
@Thickness 0.400 mm
HB
@Thickness 0.0157 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 290 °C554 °FAs Tested; Injection
Mold Temperature 100 °C212 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Xantar® LDS 3730 Polycarbonate
Mitsubishi Xantar® 19 UR Polycarbonate
Mitsubishi Xantar® 24 UR Polycarbonate
Mitsubishi Xantar® LDS 3732 Polycarbonate
Mitsubishi Xantar® LDS 3760 Polycarbonate

PMITSU9317 / 191991

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.