MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Phosphorized Admiralty Copper, UNS C44400, Cold Drawn and Annealed
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent cold workability for forming and bending.

Applications: condenser, evaporator and heat exchanger tubing, condenser tubing plates, distiller tubing, ferrules.

Key Words: Inhibited Admiralty Metal, Admiralty Brass, CDA 443, CZ111, ISO CuZn28Sn1As
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.53 g/cc0.308 lb/in³
Grain Size  15 µm
@Treatment Temp. 370 °C
15 µm
@Treatment Temp. 698 °F
cold drawn 50%, annealed 1h
 20 µm
@Treatment Temp. 400 °C
20 µm
@Treatment Temp. 752 °F
cold drawn 50%, annealed 1h
 45 µm
@Treatment Temp. 500 °C
45 µm
@Treatment Temp. 932 °F
cold drawn 50%, annealed 1h
 115 µm
@Treatment Temp. 600 °C
115 µm
@Treatment Temp. 1110 °F
cold drawn 50%, annealed 1h
 200 µm
@Treatment Temp. 700 °C
200 µm
@Treatment Temp. 1290 °F
cold drawn 50%, annealed 1h
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell F  45
@Treatment Temp. 700 °C
45
@Treatment Temp. 1290 °F
cold drawn 50%, annealed 1h
 54
@Treatment Temp. 600 °C
54
@Treatment Temp. 1110 °F
cold drawn 50%, annealed 1h
 64
@Treatment Temp. 500 °C
64
@Treatment Temp. 932 °F
cold drawn 50%, annealed 1h
 76
@Treatment Temp. 400 °C
76
@Treatment Temp. 752 °F
cold drawn 50%, annealed 1h
 97
@Treatment Temp. 300 °C
97
@Treatment Temp. 572 °F
cold drawn 50%, annealed 1h
 110
@Treatment Temp. 120 °C
110
@Treatment Temp. 248 °F
cold drawn 50%, annealed 1h
 110
@Treatment Temp. 200 °C
110
@Treatment Temp. 392 °F
cold drawn 50%, annealed 1h
Tensile Strength, Ultimate  330 MPa
@Treatment Temp. 700 °C
47900 psi
@Treatment Temp. 1290 °F
cold drawn 50%, annealed 1h
 335 MPa
@Treatment Temp. 600 °C
48600 psi
@Treatment Temp. 1110 °F
cold drawn 50%, annealed 1h
 350 MPa
@Treatment Temp. 500 °C
50800 psi
@Treatment Temp. 932 °F
cold drawn 50%, annealed 1h
 380 MPa
@Treatment Temp. 400 °C
55100 psi
@Treatment Temp. 752 °F
cold drawn 50%, annealed 1h
 455 MPa
@Treatment Temp. 300 °C
66000 psi
@Treatment Temp. 572 °F
cold drawn 50%, annealed 1h
 645 MPa
@Treatment Temp. 200 °C
93500 psi
@Treatment Temp. 392 °F
cold drawn 50%, annealed 1h
 680 MPa
@Treatment Temp. 120 °C
98600 psi
@Treatment Temp. 248 °F
cold drawn 50%, annealed 1h
Elongation at Break  5.0 %
@Treatment Temp. 120 °C
5.0 %
@Treatment Temp. 248 °F
cold drawn 50%, annealed 1h
 7.0 %
@Treatment Temp. 200 °C
7.0 %
@Treatment Temp. 392 °F
cold drawn 50%, annealed 1h
 43 %
@Treatment Temp. 300 °C
43 %
@Treatment Temp. 572 °F
cold drawn 50%, annealed 1h
 61 %
@Treatment Temp. 400 °C
61 %
@Treatment Temp. 752 °F
cold drawn 50%, annealed 1h
 70 %
@Treatment Temp. 500 °C
70 %
@Treatment Temp. 932 °F
cold drawn 50%, annealed 1h
 74 %
@Treatment Temp. 600 °C
74 %
@Treatment Temp. 1110 °F
cold drawn 50%, annealed 1h
 75 %
@Treatment Temp. 700 °C
75 %
@Treatment Temp. 1290 °F
cold drawn 50%, annealed 1h
Modulus of Elasticity 110 GPa16000 ksi
Poissons Ratio 0.380.38calculated
Fatigue Strength 115 - 125 MPa
@# of Cycles 1.00e+7
16700 - 18100 psi
@# of Cycles 1.00e+7
source does not state temper
Machinability 30 %30 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 40.0 GPa5800 ksi
Charpy Impact 82.4 J60.8 ft-lb
 79.7 J
@Temperature -18.0 °C,
Treatment Temp. 700 °C
58.8 ft-lb
@Temperature -0.400 °F,
Treatment Temp. 1290 °F
keyhole notch
 79.9 J
@Temperature -50.0 °C,
Treatment Temp. 700 °C
58.9 ft-lb
@Temperature -58.0 °F,
Treatment Temp. 1290 °F
keyhole notch
 80.3 J
@Temperature -115 °C,
Treatment Temp. 700 °C
59.2 ft-lb
@Temperature -175 °F,
Treatment Temp. 1290 °F
keyhole notch
 82.2 J
@Temperature 3.00 °C,
Treatment Temp. 700 °C
60.6 ft-lb
@Temperature 37.4 °F,
Treatment Temp. 1290 °F
keyhole notch
 82.4 J
@Temperature -30.0 °C,
Treatment Temp. 700 °C
60.8 ft-lb
@Temperature -22.0 °F,
Treatment Temp. 1290 °F
keyhole notch
 82.4 J
@Temperature 20.0 °C,
Treatment Temp. 700 °C
60.8 ft-lb
@Temperature 68.0 °F,
Treatment Temp. 1290 °F
keyhole notch
 83.4 J
@Temperature -80.0 °C,
Treatment Temp. 700 °C
61.5 ft-lb
@Temperature -112 °F,
Treatment Temp. 1290 °F
keyhole notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000690 ohm-cm
@Temperature 20.0 °C
0.00000690 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
11.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.380 J/g-°C0.0908 BTU/lb-°F
Thermal Conductivity 110 W/m-K
@Temperature 20.0 °C
763 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 900 - 935 °C1650 - 1720 °F
Solidus 900 °C1650 °F
Liquidus 935 °C1720 °F
Annealing Point 427 - 593 °C800 - 1100 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 425 - 600 °C797 - 1110 °F
Hot-Working Temperature 650 - 800 °C1200 - 1470 °F
Recrystallization Temperature 300 °C572 °FFor 1 mm strip cold rolled hard (50% reduction), from 0.015 mm grain size
 
Component Elements PropertiesMetricEnglishComments
Antimony, Sb 0.02 - 0.10 %0.02 - 0.10 %
Copper, Cu 70 - 73 %70 - 73 %
Iron, Fe <= 0.060 %<= 0.060 %
Lead, Pb <= 0.070 %<= 0.070 %
Tin, Sn 0.90 - 1.2 %0.90 - 1.2 %
Zinc, Zn 28 %28 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arsenical Admiralty Copper, UNS C44300, H04 Temper strip
Arsenical Admiralty Copper, UNS C44300
Dezincification Brass, DZR, UNS C35330
Free-Cutting Brass, UNS C36000
Mueller Alloy 3533 Dezincification Brass (UNS C35330)

MC44400c9 / 171641

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.